Self-cleaning antique brick and preparation method thereof

By forming a hydrophilic self-cleaning glaze layer with high surface tension and aging resistance on the surface of antique bricks, the problems of poor aging resistance and limited binding force of self-cleaning coatings in the prior art are solved, and the durable self-cleaning of antique bricks are achieved. and cost reduction.

CN118754724BActive Publication Date: 2024-11-26FOSHAN DONGPENG CERAMIC +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411251754.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-26
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The self-cleaning coatings of existing antique bricks have poor aging resistance and limited binding force with the brick surface, resulting in poor self-cleaning aging, and the additional coating of hydrophilic self-cleaning coatings is not conducive to reducing production costs.

Method used

A self-cleaning antique brick preparation method is adopted. After forming a bottom glaze layer on the surface of the ceramic blank, it is calcined with hydrophilic self-cleaning glaze to form a phase-separated upper layer with boron trioxide and lithium oxide, and calcium oxide and oxidation. Magnesium, aluminum trioxide, silica and potassium oxide are hydrophilic self-cleaning glaze layers in the lower phase separation layer, which improves its surface tension and binding force.

Benefits of technology

It achieves excellent, uniform and long-lasting self-cleaning performance of antique bricks, reduces production costs, and improves the aging resistance of the self-cleaning coating and its binding force with the brick surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of building ceramics, and in particular to a self-cleaning antique brick and a preparation method thereof, comprising the following steps: A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank with a concave-convex effect on the surface after drying; B. applying a base glaze on the surface of the blank to form a base glaze layer; C. preparing a hydrophilic self-cleaning glaze; D. applying the hydrophilic self-cleaning glaze on the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer; E. calcining in a kiln after drying to obtain a self-cleaning antique brick. The present invention proposes a preparation method for a self-cleaning antique brick and a preparation method thereof, which has a simple preparation method and strong operability. The obtained self-cleaning antique brick not only has excellent, uniform and lasting self-cleaning property while ensuring the appearance, but also helps to reduce costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, in particular to a self-cleaning antique brick and a preparation method thereof. Background Art

[0002] Antique tiles, as an artistic building material that combines classical aesthetics with modern craftsmanship, are deeply favored by consumers for their unique antique glaze effect, rich color layers and strong historical charm. They are widely used in home decoration, commercial places, cultural and tourist attractions and other fields.

[0003] In order to ensure the antique effect of antique tiles, the surface of antique tiles is usually designed to be uneven. Although the uneven surface is conducive to increasing its anti-slip performance, it is also easy to become a breeding ground for dirt and grime, which not only affects the aesthetics of the antique tiles and reduces its decorative effect, but also makes the treatment of dirt on antique tiles time-consuming and laborious, and requires the help of cleaning agents to be effectively removed.

[0004] In order to overcome the above-mentioned defects, the prior art usually coats the surface of the antique brick with a hydrophilic self-cleaning coating, so that a layer of hydrophilic self-cleaning coating is formed on the surface of the antique brick, so that water can spread quickly when it contacts the coating surface (that is, the static contact angle between water and the coating is small) and form a uniform water film, which can penetrate into the interface between the dirt and the coating, thereby reducing the adhesion of the dirt, and under the action of gravity, the continuously flowing water film can take away and remove the dirt on the surface of the antique brick, achieving a self-cleaning effect. However, due to the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface, the hydrophilic self-cleaning coating is easy to fall off, which is not conducive to extending the service life of the coating, resulting in poor self-cleaning durability of the coating, and it is difficult to meet actual use requirements. In addition, additionally coating the surface of the antique brick substrate with a hydrophilic self-cleaning coating is not conducive to reducing production costs. Summary of the invention

[0005] The first purpose of the present invention is to provide a self-cleaning antique brick and a preparation method thereof. The preparation method is simple and easy to operate. The obtained self-cleaning antique brick not only has excellent, uniform and lasting self-cleaning properties while ensuring the appearance, but also helps to reduce costs.

[0006] The second purpose of the present invention is to provide a self-cleaning antique brick prepared by a preparation method of the self-cleaning antique brick. The static contact angle of the self-cleaning antique brick before being soaked in boiling water is 8-15°, and the static contact angle after being soaked in boiling water for 30 days is 15-22°, and the self-cleaning antique brick has excellent, uniform and lasting self-cleaning performance.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] A method for preparing a self-cleaning antique brick comprises the following steps:

[0009] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0010] B. Applying base glaze on the surface of the body to form a base glaze layer;

[0011] Calculated by mass percentage, the chemical composition of the base glaze includes SiO257-63%, Al2O323-25%, Na2O2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO25.5-6.5%;

[0012] C. Prepare hydrophilic self-cleaning glaze;

[0013] Calculated by mass percentage, the hydrophilic self-cleaning glaze comprises 75-95% of hydrophilic frit and 5-25% of kaolin;

[0014] Calculated by mass percentage, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 2-6% kaolin, 5-8% quartz, 3-7% aluminum oxide and 14-20% leucite;

[0015] The chemical composition of the leucite includes SiO2, Al2O3 and K2O;

[0016] D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer;

[0017] E. After drying, put it into the kiln for calcination to obtain self-cleaning antique bricks.

[0018] Furthermore, in step C, the mesh size of the leucite is 200-400 meshes.

[0019] Furthermore, calculated by mass percentage, the chemical composition of the leucite includes SiO2 54-55%, Al2O3 19-20%, K2O 18-22%, Na2O 0.5-1% and CaO 0-0.5%, with the remainder being loss on ignition.

[0020] Furthermore, in step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

[0021] Furthermore, in step C, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4% by mass.

[0022] Furthermore, in step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82 to 1.9.

[0023] Furthermore, in step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

[0024] Furthermore, in step C, the calcination curve of the hydrophilic frit is: heating from room temperature to 1530° C. at a heating rate of 8 to 10° C. / min, and then keeping the temperature for 35 to 45 minutes;

[0025] In step E, the temperature of the calcination in the kiln is 1200-1220°C.

[0026] Furthermore, in step C, the preparation steps of the hydrophilic self-cleaning glaze are: mixing the raw materials of the hydrophilic frit evenly according to the ratio, calcining and quenching with water to obtain the hydrophilic frit; mixing the raw materials of the hydrophilic self-cleaning glaze evenly according to the ratio, adding sodium carboxymethyl cellulose, sodium tripolyphosphate and water for ball milling, and sieving to obtain the hydrophilic self-cleaning glaze.

[0027] A self-cleaning antique brick is prepared by using the self-cleaning antique brick preparation method. The static contact angle of the self-cleaning antique brick before being soaked in boiling water is 8-15 degrees, and the static contact angle after being soaked in boiling water for 30 days is 15-22 degrees.

[0028] The technical solution provided by the present invention may include the following beneficial effects:

[0029] 1. In the early stage of sintering, the hydrophilic frit formula system has achieved phase separation, and boric acid and lithium carbonate are the upper phase separation layer, and the second gradient flux system (wollastonite and calcined talc) and high-temperature raw materials (kaolin, quartz, aluminum oxide and leucite) are the lower phase separation layer. When the calcination temperature reaches the melting point of each raw material in the lower phase separation layer, each raw material in the lower phase separation layer will also gradually melt. Further, as the calcination temperature rises again, each raw material in the upper phase separation layer and the lower phase separation layer will gradually decompose, so that the hydrophilic frit will eventually form a phase separation melt with boron trioxide and lithium oxide as the upper phase separation layer, and calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide and potassium oxide as the lower phase separation layer. When the hydrophilic frit, which is essentially a phase-separated melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze will form, after calcination, a hydrophilic self-cleaning glaze layer with boron trioxide and lithium oxide components as the phase-separated upper layer and calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide and potassium oxide components as the phase-separated lower layer.

[0030] 2. Since the surface tension of lithium oxide is 450×10 -3 N / M, the surface tension of boron oxide is 80×10 -3 N / M, while the surface tension of water is 73×10 -3N / m, that is, the surface tension of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of water, so that the surface of the hydrophilic self-cleaning glaze layer has extremely strong hydrophilic self-cleaning performance, even if the surface of the hydrophilic self-cleaning glaze layer is adhered with dirt, the dirt is relatively easy to be removed. In addition, compared with the hydrophilic self-cleaning coating, the aging resistance of the hydrophilic self-cleaning glaze layer is greatly improved, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the poor aging resistance of the hydrophilic self-cleaning coating in the prior art. Further, since the hydrophilic self-cleaning glaze layer is directly calcined by the hydrophilic self-cleaning glaze, its bonding force with the antique brick is extremely high, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the limited bonding force between the hydrophilic self-cleaning coating and the brick surface of the antique brick in the prior art. The mutual coordination of the above multiple factors is conducive to realizing the long-lasting self-cleaning of the antique brick, and the self-cleaning is excellent. In addition, the technical solution does not need to additionally apply the hydrophilic self-cleaning coating on the surface of the antique brick, which is conducive to saving production costs and improving production efficiency.

[0031] 3. If no leucite is added to the hydrophilic frit formula, when the hydrophilic self-cleaning glaze is calcined to form a phase-separated lower layer with calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide as components, it does not contain potassium oxide (which can greatly reduce its surface tension), so that the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of the bottom glaze layer. The surface tension between the phase-separated lower layer and the bottom glaze layer of the hydrophilic self-cleaning glaze layer is extremely different, which makes the hydrophilic self-cleaning glaze layer prone to glaze shrinkage, and the hydrophilic self-cleaning glaze layer obtained after calcination is prone to shrinkage holes, and the bottom glaze layer is partially exposed, which not only easily affects the uniformity of the hydrophilic self-cleaning property, but also easily affects the appearance of the product. DETAILED DESCRIPTION

[0032] The present technical solution provides a method for preparing a self-cleaning antique brick, comprising the following steps:

[0033] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0034] B. Applying base glaze on the surface of the body to form a base glaze layer;

[0035] Calculated by mass percentage, the chemical composition of the base glaze includes SiO257-63%, Al2O323-25%, Na2O2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO25.5-6.5%;

[0036] C. Prepare hydrophilic self-cleaning glaze;

[0037] Calculated by mass percentage, the hydrophilic self-cleaning glaze comprises 75-95% of hydrophilic frit and 5-25% of kaolin;

[0038] Calculated by mass percentage, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 2-6% kaolin, 5-8% quartz, 3-7% aluminum oxide and 14-20% leucite;

[0039] The chemical composition of the leucite includes SiO2, Al2O3 and K2O;

[0040] D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer;

[0041] E. After drying, put it into the kiln for calcination to obtain self-cleaning antique bricks.

[0042] The prior art usually coats the surface of the antique brick substrate with a hydrophilic self-cleaning coating, so that a layer of hydrophilic self-cleaning coating is formed on the surface of the antique brick, so that even if there is dirt on the surface of the antique brick, the dirt can be easily removed. However, due to the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface, the hydrophilic self-cleaning coating is easy to fall off, which is not conducive to extending the service life of the coating, resulting in poor self-cleaning durability of the coating, and it is difficult to meet the actual use requirements. In addition, additionally coating the surface of the antique brick substrate with a hydrophilic self-cleaning coating is not conducive to reducing production costs.

[0043] First, in order to achieve long-lasting self-cleaning properties under the premise of reducing costs, the technical solution proposes a hydrophilic self-cleaning glaze, the raw materials of which include hydrophilic frit and kaolin. Among them, the hydrophilic frit uses boric acid, lithium carbonate, wollastonite and calcined talc as fluxes, and the melting point of boric acid is about 577°C, the melting point of lithium carbonate is about 723°C, the melting point of wollastonite is about 1500°C, and the melting point of calcined talc is about 1400°C, so that the hydrophilic frit formula forms a first gradient fluxing system composed of boric acid and lithium carbonate, and a second gradient fluxing system composed of wollastonite and calcined talc, and the melting temperatures of the two gradient fluxing systems are extremely different.

[0044] Since the melting temperatures of the first gradient fluxing system and the high-temperature raw materials in the hydrophilic frit formula (i.e., the raw materials that form the solid phase, such as kaolin, quartz, alumina and leucite, among which the melting temperature of kaolin is about 1780℃, the melting temperature of quartz is about 1713℃, the melting temperature of alumina is 2054℃, and the melting temperature of leucite is about 1698℃) are quite different, and the melting temperatures of the high-temperature raw materials in the second gradient fluxing system and the hydrophilic frit formula are relatively different, the raw materials of the first gradient fluxing system melt first in the early stage of firing of the tile, so that the hydrophilic frit obtains a melt mainly composed of boric acid and lithium carbonate in the early stage of calcination. As the calcination temperature increases, the melt viscosity gradually decreases, and other raw materials that are far from reaching the melting point (such as the raw materials of the second gradient fluxing system and the high-temperature raw materials) will sink. That is, in the early stage of firing, the hydrophilic frit formula system has achieved phase separation, and boric acid and lithium carbonate are the upper phase separation layer, and the second gradient flux system (wollastonite and calcined talc) and high-temperature raw materials (kaolin, quartz, aluminum oxide and leucite) are the lower phase separation layer. When the calcination temperature reaches the melting point of each raw material in the lower phase separation layer, each raw material in the lower phase separation layer will also gradually melt. Further, as the calcination temperature rises again, each raw material in the upper phase separation layer and the lower phase separation layer will gradually decompose, so that the hydrophilic frit will eventually form a phase separation melt with boron trioxide and lithium oxide components as the upper phase separation layer, and calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide and potassium oxide components as the lower phase separation layer.

[0045] When the hydrophilic frit, which is essentially a phase-separated melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze will form, after calcination, a hydrophilic self-cleaning glaze layer with boron trioxide and lithium oxide components as the phase-separated upper layer and calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide and potassium oxide components as the phase-separated lower layer.

[0046] Furthermore, since the surface tension of lithium oxide is 450×10 -3 N / M, the surface tension of boron oxide is 80×10 - 3 N / M, while the surface tension of water is 73×10 -3N / m, that is, the surface tension of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of water, so that the surface of the hydrophilic self-cleaning glaze layer has extremely strong hydrophilic self-cleaning performance, even if the surface of the hydrophilic self-cleaning glaze layer is adhered with dirt, the dirt is relatively easy to be removed. In addition, compared with the hydrophilic self-cleaning coating, the aging resistance of the hydrophilic self-cleaning glaze layer is greatly improved, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the poor aging resistance of the hydrophilic self-cleaning coating in the prior art. Further, since the hydrophilic self-cleaning glaze layer is directly calcined by the hydrophilic self-cleaning glaze, its bonding force with the antique brick is extremely high, which is conducive to overcoming the technical defects of poor self-cleaning timeliness due to the limited bonding force between the hydrophilic self-cleaning coating and the brick surface of the antique brick in the prior art. The mutual coordination of the above multiple factors is conducive to realizing the long-lasting self-cleaning of the antique brick, and the self-cleaning is excellent. In addition, the technical solution does not need to additionally apply the hydrophilic self-cleaning coating on the surface of the antique brick, which is conducive to saving production costs and improving production efficiency.

[0047] Furthermore, in order to ensure the fluxing effect and the expansion coefficient is compatible with the expansion coefficient of the body, potassium feldspar and sodium feldspar are usually added to the base glaze formula, and the chemical components of the existing base glaze include silicon dioxide, aluminum oxide, sodium oxide, calcium oxide, potassium oxide and zirconium oxide. When the hydrophilic frit, which is essentially a phase-separated melt, is added to the hydrophilic self-cleaning glaze formula, the hydrophilic self-cleaning glaze is calcined to form a hydrophilic self-cleaning glaze layer with calcium oxide, magnesium oxide, aluminum oxide, silicon dioxide and potassium oxide as the phase-separated lower layer. That is, the chemical composition of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the chemical composition of the base glaze layer both contain silicon dioxide, aluminum oxide, calcium oxide and potassium oxide (the surface tension of calcium oxide is 470×10 -3 N / M, the surface tension of silicon dioxide is 290×10 -3 N / M, the surface tension of aluminum oxide is 380×10 -3 N / M, the surface tension of potassium oxide is 10×10 -3 N / M), and the lower layer of the hydrophilic self-cleaning glaze layer also contains magnesium oxide, while the bottom glaze layer also contains zirconium oxide and sodium oxide. Among them, the surface tension of magnesium oxide is 545×10 -3 N / M, the surface tension of zirconium oxide is 410×10 -3 N / M, the surface tension of sodium oxide is 150×10 -3N / M, although the surface tension of magnesium oxide is greater than that of zirconium oxide and sodium oxide, since both the phase-separated lower layer and the bottom glaze layer of the hydrophilic self-cleaning glaze layer contain potassium oxide which can greatly reduce the surface tension of the two, the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the bottom glaze layer is matched, thereby avoiding the great difference in surface tension between the phase-separated lower layer and the bottom glaze layer of the hydrophilic self-cleaning glaze layer, which leads to the phenomenon of glaze shrinkage in the hydrophilic self-cleaning glaze layer, and the hydrophilic self-cleaning glaze layer obtained after calcination is prone to shrinkage holes, and the bottom glaze layer is partially exposed, which not only easily affects the uniformity of the hydrophilic self-cleaning property, but also easily affects the appearance of the product.

[0048] It should be noted that after the hydrophilic self-cleaning glaze separates into phases during the calcination process, a large amount of liquid phase will appear in the upper and lower layers of the phase separation, and the composition difference between the upper and lower layers of the phase separation is also relatively large, which makes it easy for ions to exchange between the upper and lower layers of the phase separation and form an intermediate layer. The existence of the intermediate layer will shorten the difference in surface tension between the upper and lower layers of the phase separation, so that even if there is a large tension difference between the upper and lower layers of the phase separation, the glaze shrinkage phenomenon will not occur inside the hydrophilic self-cleaning glaze layer.

[0049] In addition, in order to ensure the effects of sealing and whitening, the existing base glaze contains more zirconium dioxide in its chemical composition, and the amount of fluxing components added is relatively small (the sum of the amount of fluxing components potassium oxide, sodium oxide and calcium oxide added is 8.7-10.3%), which greatly reduces the amount of liquid phase produced during the calcination process relative to the amount of liquid phase produced during the calcination process of the hydrophilic self-cleaning glaze, resulting in a greatly reduced ion exchange efficiency between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze, and the intermediate layer formed between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze is thinner, and its composition is closer to the phase-separated lower layer of the hydrophilic self-cleaning glaze, making it difficult to close the difference in surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze and the base glaze. Therefore, when the surface tension between the phase-separated lower layer of the hydrophilic self-cleaning glaze layer and the base glaze layer is extremely different, the hydrophilic self-cleaning glaze layer is prone to glaze shrinkage.

[0050] Secondly, if no white garnet is added to the hydrophilic frit formula, when the hydrophilic self-cleaning glaze is calcined to form a phase-separated lower layer with calcium oxide, magnesium oxide, aluminum oxide and silicon dioxide as components, it does not contain potassium oxide (which can greatly reduce its surface tension), so that the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer is much greater than the surface tension of the bottom glaze layer. The surface tension between the phase-separated lower layer and the bottom glaze layer of the hydrophilic self-cleaning glaze layer is extremely different, which makes the hydrophilic self-cleaning glaze layer prone to glaze shrinkage, and the hydrophilic self-cleaning glaze layer obtained after calcination is prone to shrinkage holes, and the bottom glaze layer is partially exposed, which not only easily affects the uniformity of the hydrophilic self-cleaning property, but also easily affects the appearance of the product.

[0051] In addition, the technical solution cannot use potassium feldspar to replace white garnet, nor can potassium feldspar and / or sodium feldspar be added to the hydrophilic frit as flux. The reason is that the melting point of potassium feldspar is about 1150°C and the melting point of sodium feldspar is about 1120°C. When potassium feldspar and / or sodium feldspar are added to the hydrophilic frit formula, the melting temperature difference between the first gradient fluxing system and the second gradient fluxing system will be greatly reduced, resulting in the inability of the formula system to achieve phase separation. At the same time, since potassium feldspar and sodium feldspar contain a large amount of aluminum oxide and silicon dioxide components, the high-temperature viscosity of the early melt will not drop significantly, further resulting in the inability of the formula system to achieve phase separation. In addition, the potassium oxide produced during the calcination of potassium feldspar and the sodium oxide produced during the calcination of sodium feldspar have a surface tension that is smaller than the surface tension of water, that is, when potassium feldspar and / or sodium feldspar are added to the formula, it is not conducive to the self-cleaning property of the hydrophilic self-cleaning glaze.

[0052] Again, the introduction of boric acid in the technical solution, in addition to effectively promoting the phase separation of the hydrophilic self-cleaning glaze during the calcination process, is also conducive to inhibiting the hydrophilic self-cleaning glaze from crystallizing in the intermediate layer between the two phase-separated melts of the phase-separated upper layer and the phase-separated lower layer during calcination, thereby avoiding the liquid phase of the phase-separated upper layer being too low, resulting in the unstable self-cleaning performance of the hydrophilic self-cleaning glaze. In addition, the kaolin, quartz and alumina in the hydrophilic frit are not only conducive to improving the hardness, wear resistance and other properties of the hydrophilic frit, but the above three raw materials are all high-temperature raw materials, which are conducive to improving the temperature difference between the upper raw materials and the lower raw materials in the hydrophilic frit, and promoting the glaze to be phase-separated in the early stage of firing. It should be noted that the kaolin in the hydrophilic self-cleaning glaze formula of the technical solution is mainly used as a suspending agent to avoid the hydrophilic frit settling and affecting its performance.

[0053] Finally, according to the mass percentage, the hydrophilic frit includes 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 2-6% kaolin, 5-8% quartz, 3-7% aluminum oxide and 14-20% leucite. That is, the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and calcined talc is 1:(3-8). When the ratio is greater than 1:3, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination will be too much, the fluxing effect will be too strong, and the solid phase raw materials that are difficult to melt in the early stage will be easily melted, resulting in difficulty in phase separation; when the ratio is less than 1:8, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination will be too small, which will make it difficult for the second gradient fluxing system and high-temperature raw materials to sink, resulting in difficulty in phase separation; on the other hand, the liquid phase on the upper layer of the phase separation will be too thin, affecting the surface tension of the glaze, and thus affecting its self-cleaning hydrophilic properties.

[0054] Furthermore, when the addition amount of white garnet in the hydrophilic frit is less than 14%, the potassium oxide content in the lower phase layer of the hydrophilic self-cleaning glaze layer will be too low, so that the surface tension of the lower phase layer of the hydrophilic self-cleaning glaze layer is still much larger than the surface tension of the bottom glaze layer, and the surface tension of the lower phase layer in the hydrophilic self-cleaning glaze layer does not match the surface tension of the bottom glaze layer, resulting in glaze shrinkage on the glaze surface; when the addition amount of white garnet is greater than 20%, the potassium oxide content in the lower phase layer of the hydrophilic self-cleaning glaze layer is too high, resulting in the surface tension of the lower phase layer of the hydrophilic self-cleaning glaze layer is too small, and the surface tension of the lower phase layer of the hydrophilic self-cleaning glaze layer is much smaller than the surface tension of the bottom glaze layer, and the surface tension of the lower phase layer in the hydrophilic self-cleaning glaze layer does not match the surface tension of the bottom glaze layer, resulting in glaze flow defects on the glaze surface.

[0055] Preferably, calculated by mass percentage, the hydrophilic self-cleaning glaze includes 80% hydrophilic frit and 20% kaolin; calculated by mass percentage, the hydrophilic frit includes 4% boric acid, 8% lithium carbonate, 38% wollastonite, 13% talc, 6% kaolin, 8% quartz, 5% alumina and 18% leucite.

[0056] Preferably, the base glaze includes the following raw materials in parts by mass: 30-40 parts of potassium feldspar, 10-15 parts of sodium feldspar, 3-10 parts of washed kaolin, 10-30 parts of calcined kaolin, 5-15 parts of quartz, 5-15 parts of calcined alumina, 3-5 parts of talc, 2-6 parts of limestone and 5-15 parts of zirconium silicate. But it is not limited thereto.

[0057] Further description, in step C, the mesh size of the leucite is 200-400 mesh.

[0058] The technical solution preferably adds white garnet with a mesh size of 200 to 400 meshes to the formula. On the one hand, it is easy to mix it with other raw materials to ensure its uniform dispersion; on the other hand, the white garnet with a mesh size of 200 to 400 meshes has larger particles, which is conducive to its sinking when it is far from reaching the melting point as the calcination temperature increases and the melt viscosity decreases, thereby promoting phase separation and ensuring the performance of the hydrophilic self-cleaning glaze.

[0059] It is further explained that, calculated by mass percentage, the chemical composition of the white garnet includes SiO2 54-55%, Al2O3 19-20%, K2O 18-22%, Na2O 0.5-1% and CaO 0-0.5%, and the rest is loss on ignition.

[0060] The technical solution preferably adds white garnet with a K2O content of 18-22% calculated by mass percentage to the hydrophilic frit raw material, which helps to increase the K2O content in the formula to reduce the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer, and make the surface tension of the phase-separated lower layer of the hydrophilic self-cleaning glaze layer match the surface tension of the base glaze layer to ensure the performance of the product.

[0061] It is further described that in step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

[0062] Optimizing the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and calcined talc is helpful to promote the phase separation of the hydrophilic self-cleaning glaze in the early stage of calcination, thereby ensuring the performance of the hydrophilic self-cleaning glaze.

[0063] Further, in step C, according to the mass percentage, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4%.

[0064] By limiting the fineness of the hydrophilic self-cleaning glaze, the sieve residue of the hydrophilic self-cleaning glaze is low, which is beneficial to making the hydrophilic self-cleaning glaze have fine uniformity, reducing the rough glaze surface caused by uneven particles, and improving the self-cleaning performance.

[0065] Further, in step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82-1.9.

[0066] When the specific gravity of the hydrophilic self-cleaning glaze is too high, the glaze will be too thick and the fluidity will be poor, which will make the application uniformity of the hydrophilic self-cleaning glaze poor and easily form defects such as glaze path. In addition, the specific gravity of the hydrophilic self-cleaning glaze is too high, which will easily hinder the discharge of gas and water generated during the calcination process of the hydrophilic self-cleaning glaze, causing the glaze layer obtained by calcining the hydrophilic self-cleaning glaze to crack easily.

[0067] When the specific gravity of the hydrophilic self-cleaning glaze is too low, the fluidity of the hydrophilic self-cleaning glaze is too good, and it is easy to flow during the glazing process, which also leads to poor uniformity of the hydrophilic self-cleaning glaze and easy formation of defects such as glaze paths. In addition, the specific gravity of the hydrophilic self-cleaning glaze is too low, resulting in excessive water in the glaze, which is prone to brick explosion during the calcination process.

[0068] It should be noted that glaze path means that the glaze layer is thicker in some areas and thinner or missing in other areas.

[0069] Further, in step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

[0070] By limiting the glazing thickness, it is beneficial to ensure that the melt mainly composed of boric acid and lithium carbonate has a certain thickness in the early stage of calcination, so that the raw materials that have not yet reached the melting point have enough space to sink, thereby promoting phase separation and ensuring its performance.

[0071] Further, in step C, the calcination curve of the hydrophilic frit is: heating from room temperature to 1530°C at a heating rate of 8-10°C / min, and then keeping the temperature for 35-45min;

[0072] In step E, the temperature of calcining in the kiln is 1200-1220°C.

[0073] By optimizing the calcination curve of the hydrophilic frit, all raw materials in the hydrophilic frit formula can be melted, which is conducive to promoting phase separation, ensuring the performance of the hydrophilic frit, and making the hydrophilic self-cleaning glaze with the addition of hydrophilic frit have a certain sense of transparency after calcination, thereby improving its permeability.

[0074] In addition, by limiting the glaze firing temperature to 1200-1220°C, which is consistent with the firing temperature of existing antique tile products, it is easy to achieve the purpose of industrialized production while ensuring product performance and reducing large deviations between the experimental stage and the industrialization stage.

[0075] Further explanation, in step C, the preparation steps of the hydrophilic self-cleaning glaze are: mixing the raw materials of the hydrophilic frit evenly according to the ratio, calcining and quenching with water to obtain the hydrophilic frit; mixing the raw materials of the hydrophilic self-cleaning glaze evenly according to the ratio, adding sodium carboxymethyl cellulose, sodium tripolyphosphate and water for ball milling, and sieving to obtain the hydrophilic self-cleaning glaze.

[0076] The technical scheme also proposes a preparation method for a hydrophilic self-cleaning glaze, which is simple and easy to operate. Preferably, calculated by mass percentage, the amount of sodium carboxymethyl cellulose added is 0.2% of the amount of dry material added to the hydrophilic self-cleaning glaze, the amount of sodium tripolyphosphate added is 0.3% of the amount of dry material added to the hydrophilic self-cleaning glaze, and the amount of water added is 35-38% of the amount of dry material added to the hydrophilic self-cleaning glaze. After adding the above additives to the mixed material, ball milling is performed for 12 hours, and then sieving is performed to obtain the hydrophilic self-cleaning glaze.

[0077] A self-cleaning antique brick is prepared by using the self-cleaning antique brick preparation method. The static contact angle of the self-cleaning antique brick before being soaked in boiling water is 8-15 degrees, and the static contact angle after being soaked in boiling water for 30 days is 15-22 degrees.

[0078] A self-cleaning antique brick prepared by the preparation method of the self-cleaning antique brick has a static contact angle of 8-15° before being soaked in boiling water and a static contact angle of 15-22° after being soaked in boiling water for 30 days, and has excellent, uniform and lasting self-cleaning performance.

[0079] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0080] Performance Test:

[0081] Appearance: Observe the glaze surface of the antique tile with the naked eye.

[0082] Static contact angle before immersion: According to the test method of "GB / T 30447-2013 Nanofilm Contact Angle Measurement Method", the static contact angle of the hydrophilic self-cleaning antique tile before immersion in boiling water is tested. If the static contact angle is <15°, it is qualified.

[0083] Static contact angle after immersion: According to the test method of "GB / T 30447-2013 Nanofilm Contact Angle Measurement Method", the hydrophilic self-cleaning antique tiles are tested for their static contact angle after being immersed in boiling water for 30 days. If the contact angle is less than 25°, it is qualified.

[0084] Anti-slip performance: Anti-slip performance is tested according to the DIN 51130:2014 anti-slip standard.

[0085] Mohs hardness: The Mohs hardness of the hydrophilic self-cleaning antique tile is tested using a Mohs hardness tester.

[0086] Example 1

[0087] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0088] B. Applying a base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO259%, Al2O325%, Na2O33%, CaO0.6%, K2O6% and ZrO26.4%;

[0089] C. 4% boric acid, 8% lithium carbonate, 38% wollastonite, 13% calcined talc, 6% kaolin, 8% quartz, 5% aluminum oxide and 18% leucite of 300 mesh are mixed evenly, calcined and water-quenched to obtain a hydrophilic frit; 80% of the hydrophilic frit and 20% kaolin are mixed evenly, sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and sieved to obtain a hydrophilic self-cleaning glaze with a specific gravity of 1.86; wherein, calculated by mass percentage, the chemical composition of the leucite includes SiO2 54.2%, Al2O3 19.4%, K2O2 1.6%, Na2O 0.5% and CaO 0.1%, and the rest is the loss on ignition; according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the residue is 0.2%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 35% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: from room temperature to 1530℃ at a heating rate of 8-10℃ / min, and then keep warm for 40min;

[0090] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.5 mm;

[0091] E. After drying, calcine at a temperature of 1200-1220°C to obtain self-cleaning antique tiles.

[0092] Example 2

[0093] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0094] B. Applying base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO262%, Al2O323%, Na2O 2.5%, CaO 0.5%, K2O 6.5% and ZrO25.5%;

[0095] C. 3% boric acid, 9% lithium carbonate, 36% wollastonite, 13% calcined talc, 4% kaolin, 8% quartz, 7% aluminum oxide and 20% leucite of 200 mesh are mixed evenly according to a ratio, and the mixture is calcined and quenched with water to obtain a hydrophilic frit; 95% of the hydrophilic frit and 5% of kaolin are mixed evenly according to a ratio, and sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and the mixture is sieved to obtain a hydrophilic self-cleaning glaze with a specific gravity of 1.9; wherein, the chemical components of the leucite include SiO2 54.8%, Al2O3 19.6%, K2O 20.3%, Na2O 0.8% and CaO 0. 0.2%, and the rest is the loss on ignition; according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the residue is 0.3%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 36% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: from room temperature to 1530℃ at a heating rate of 8-10℃ / min, and then keep warm for 45min;

[0096] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.3 mm;

[0097] E. After drying, calcine at a temperature of 1200-1220°C to obtain self-cleaning antique tiles.

[0098] Example 3

[0099] A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying;

[0100] B. Applying a base glaze on the surface of the body to form a base glaze layer; calculated by mass percentage, the chemical composition of the base glaze includes SiO2 60%, Al2O3 24%, Na2O 3.5%, CaO 0.3%, K2O 6.2% and ZrO 26%;

[0101] C. 2% boric acid, 7% lithium carbonate, 37% wollastonite, 15% calcined talc, 6% kaolin, 8% quartz, 7% aluminum oxide and 18% leucite of 400 mesh are mixed evenly according to a ratio, and then calcined and quenched with water to obtain a hydrophilic frit; 90% of the hydrophilic frit and 10% of kaolin are mixed evenly according to a ratio, and then sodium carboxymethyl cellulose, sodium tripolyphosphate and water are added for ball milling, and a hydrophilic self-cleaning glaze with a specific gravity of 1.82 to 1.9 is obtained by sieving; wherein, calculated by mass percentage, the chemical composition of the leucite includes SiO2 54.2%, Al2O3 19.8%, K2O 21.4%, Na2O 0.6% and CaO 0.3%, and the rest is the loss on ignition; according to the mass percentage, the hydrophilic self-cleaning glaze passes through a 325-mesh sieve, and the sieve residue is 0.4%; according to the mass percentage, the addition amount of sodium carboxymethyl cellulose is 0.2% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, the addition amount of sodium tripolyphosphate is 0.3% of the addition amount of the dry material of the hydrophilic self-cleaning glaze, and the addition amount of water is 38% of the addition amount of the dry material of the hydrophilic self-cleaning glaze; the calcination curve of the hydrophilic frit is: from room temperature to 1530℃ at a heating rate of 8-10℃ / min, keep warm for 35min;

[0102] D. applying a hydrophilic self-cleaning glaze to the surface of the bottom glaze layer to form a hydrophilic self-cleaning glaze layer; wherein the glazing thickness of the hydrophilic self-cleaning glaze is 0.7 mm;

[0103] E. After drying, calcine at a temperature of 1200-1220°C to obtain self-cleaning antique tiles.

[0104] Comparative Example 1

[0105] The self-cleaning antique brick in Comparative Example 1 includes an antique brick substrate and a hydrophilic self-cleaning coating distributed from bottom to top; wherein the hydrophilic self-cleaning coating is obtained by curing a super hydrophilic coating of model SM-TM-QS3500 / 3200 produced by Shangmeng Technology Wuxi Co., Ltd.

[0106] Comparative Example 2

[0107] Comparative Example 2 has the same preparation method and raw materials as Example 1, except that potassium feldspar and sodium feldspar are added to the hydrophilic frit formula in Comparative Example 2. That is, in Comparative Example 1, the hydrophilic frit includes 4% boric acid, 8% lithium carbonate, 5% potassium feldspar, 3% sodium feldspar, 38% wollastonite, 13% calcined talc, 2% kaolin, 5% quartz, 5% alumina and 17% leucite, calculated by mass percentage.

[0108] Comparative Example 3

[0109] The preparation method and raw materials of Comparative Example 3 are the same as those of Example 1, except that in Comparative Example 3, calculated by mass ratio, the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is 1:2.

[0110] Comparative Example 4

[0111] The preparation method and raw materials of Comparative Example 4 are the same as those of Example 1, except that in Comparative Example 4, the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is 1:9.

[0112] Comparative Example 5

[0113] Comparative Example 5 has the same preparation method and raw materials as Example 1, except that leucite is not added to the hydrophilic frit formula in Comparative Example 5. That is, in Comparative Example 1, the hydrophilic frit includes 4% boric acid, 8% lithium carbonate, 38% wollastonite, 13% calcined talc, 15% kaolin, 14% quartz and 7% alumina, calculated by mass percentage.

[0114] The performance tests of the self-cleaning antique tiles prepared by the preparation methods of Examples 1-3 and Comparative Examples 1-5 were respectively carried out, and the results are shown in Table 1 below:

[0115] Table 1 Performance test results of different self-cleaning antique tiles in the embodiments and comparative examples

[0116]

[0117] It can be seen from the performance test results in Table 1 that the antique brick glaze obtained by the technical solution has no shrinkage holes, the bottom glaze layer is not exposed, the static contact angle before immersion is 8-15°, and the static contact angle after immersion is 15-22°. On the premise of ensuring the appearance, it not only has excellent, uniform and lasting self-cleaning performance, but also has good anti-slip and hardness, and is both decorative and practical, which is more conducive to meeting the use needs of consumers.

[0118] In Comparative Example 1, a hydrophilic self-cleaning coating is provided on the surface of the antique brick substrate to obtain a self-cleaning antique brick. Although the obtained antique brick has a small static contact angle with water before immersion and has good self-cleaning property, it is affected by the poor aging resistance of the hydrophilic self-cleaning coating and its limited bonding force with the brick surface. As a result, after immersion, the hydrophilic self-cleaning coating of the self-cleaning antique brick in Comparative Example 1 falls off, the self-cleaning durability is poor, and the static contact angle after immersion cannot be measured.

[0119] In Comparative Example 2, since potassium feldspar and sodium feldspar are added to the hydrophilic frit formula, not only does it make phase separation difficult, but the surface tension of the hydrophilic self-cleaning glaze layer obtained by calcining the hydrophilic self-cleaning glaze is reduced, the static contact angle of the antique tile is increased, and its self-cleaning property is reduced.

[0120] In Comparative Example 3, since the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is too large, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination is too large, and the fluxing effect is too strong, which easily melts the solid phase raw materials that are difficult to melt in the early stage, resulting in difficulty in phase separation, which increases the static contact angle of the antique tile and reduces its self-cleaning property.

[0121] In Comparative Example 4, since the ratio of the sum of the mass percentages of boric acid and lithium carbonate to the sum of the mass percentages of wollastonite and talc is too small, the amount of liquid phase formed by boric acid and lithium carbonate in the melt in the early stage of calcination is too small. On the one hand, it makes it difficult for the second gradient fluxing system and the high-temperature raw materials in the hydrophilic melt to sink, resulting in difficulty in phase separation; on the other hand, it makes the liquid phase in the upper layer of the phase separation too thin, affecting the surface tension of the glaze and further affecting its self-cleaning performance.

[0122] In Comparative Example 5, due to the lack of addition of white pomegranate, shrinkage holes appeared on the glaze surface and the bottom glaze layer was partially exposed, which not only affected the appearance of the product, but also resulted in poor self-cleaning properties at the exposed part of the bottom glaze layer, affecting the self-cleaning uniformity of the product.

[0123] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing a self-cleaning antique brick, characterized in that: The following steps are involved: A. preparing a ceramic blank, pressing the ceramic blank, and obtaining a blank having a concave-convex effect on the surface after drying; B. Applying base glaze on the surface of the body to form a base glaze layer; Calculated by mass percentage, the chemical composition of the base glaze includes SiO2 57-63%, Al2O3 23-25%, Na2O2.5-3.5%, CaO 0.2-0.8%, K2O 6-7% and ZrO2 5.5-6.5%; C. Prepare hydrophilic self-cleaning glaze; Calculated by mass percentage, the raw materials of the hydrophilic self-cleaning glaze are 75-95% of hydrophilic frit and 5-25% of kaolin; Calculated by mass percentage, the raw materials of the hydrophilic frit are 2-4% boric acid, 5-9% lithium carbonate, 30-40% wollastonite, 9-16% calcined talc, 2-6% kaolin, 5-8% quartz, 3-7% aluminum oxide and 14-20% leucite; Calculated by mass percentage, the chemical composition of the leucite includes SiO2 54-55%, Al2O3 19-20%, K2O18-22%, Na2O 0.5-1% and CaO 0-0.5%, and the rest is loss on ignition; The calcination curve of the hydrophilic frit is: heating from room temperature to 1530°C at a heating rate of 8-10°C / min, and then keeping the temperature for 35-45min; D. applying a hydrophilic self-cleaning glaze material to the surface of the base glaze layer to form a hydrophilic self-cleaning glaze layer; E. After drying, the bricks are put into a kiln for calcination to obtain self-cleaning antique bricks; the temperature of the kiln for calcination is 1200-1220°C.

2. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step C, the mesh size of the leucite is 200-400 meshes.

3. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step C, the ratio of the sum of the mass percentages of the boric acid and the lithium carbonate to the sum of the mass percentages of the wollastonite and the calcined talc is 1:(4-7).

4. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step C, the hydrophilic self-cleaning glaze is passed through a 325-mesh sieve, and the residue is 0.2-0.4% by mass.

5. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step C, the specific gravity of the hydrophilic self-cleaning glaze is 1.82-1.

9.

6. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step D, the glazing thickness of the hydrophilic self-cleaning glaze is 0.3-0.7 mm.

7. The method for preparing a self-cleaning antique tile according to claim 1, characterized in that: In step C, the preparation steps of the hydrophilic self-cleaning glaze are: mixing the raw materials of the hydrophilic frit evenly according to the ratio, calcining and quenching with water to obtain the hydrophilic frit; mixing the raw materials of the hydrophilic self-cleaning glaze evenly according to the ratio, adding sodium carboxymethyl cellulose, sodium tripolyphosphate and water for ball milling, and sieving to obtain the hydrophilic self-cleaning glaze.

8. A self-cleaning antique brick, characterized by: The self-cleaning antique brick is prepared by the preparation method of any one of claims 1 to 7. The static contact angle of the self-cleaning antique brick before being soaked in boiling water is 8 to 15 degrees, and the static contact angle after being soaked in boiling water for 30 days is 15 to 22 degrees.