A kind of heat-stable inner tube material and preparation method thereof
Through the mixing vulcanization technology of premodified silicon nitride and modified lignin and natural rubber, the problem of degradation of inner tube materials under high temperature conditions is solved, the thermal stability, flame retardant and anti-aging performance are improved, and the thermal stability, flame retardant and anti-aging performance are improved. Overall performance of inner tube material.
Patent Information
- Application Number
- CN202411239328.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The performance of existing inner tube materials deteriorates under high temperature conditions, affecting the comfort and safety of driving and riding.
Premodified silicon nitride and modified lignin are used for mixing and vulcanization with natural rubber to form a thermally stable inner tube material. The flame retardant performance is improved by introducing Si-O bonds, amino groups and DOPO structures, and the modified lignin is introduced into maleyl The formation of a crosslinking network of imine groups improves anti-aging performance.
It significantly improves the thermal stability, flame retardant properties, corrosion resistance and aging resistance of the inner tube material, reduces the thermal expansion coefficient, enhances the thermal conductivity, and improves the overall performance of the material.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, in particular to a thermally stable inner tube material and a preparation method thereof. Background Art
[0002] The inner tube, also known as the inner tube, is the main component of tires for cars, motorcycles, bicycles, etc. The inner tube plays a very important role. It can maintain the internal pressure of the tire, thereby maintaining the shape and stability of the tire; as a part of the tire, the inner tube supports the weight of the vehicle body together with the tire to ensure that the vehicle can run smoothly; the softness of the inner tube can absorb the bumps on the road, reduce vibration, and improve driving comfort; the existence of the inner tube helps to maintain the stability of the tire and prevent the tire from deforming or rupturing due to insufficient air pressure during driving, thereby improving driving safety.
[0003] Common inner tube materials include butyl rubber, natural rubber, latex and polyurethane. When the vehicle is running, the tire will generate heat due to friction with the ground, which will generate a lot of heat. Excessive temperature will cause the overall performance of the inner tube to decline, affecting the comfort and safety of driving and riding. Therefore, it is necessary to invent an inner tube material with excellent thermal stability to improve the stability of the inner tube at high temperatures, thereby improving the safety and comfort of driving and riding. Summary of the invention
[0004] The object of the present invention is to provide a heat-stable inner tube material and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A heat-stable inner tube material, wherein the heat-stable inner tube material is prepared by reacting pre-modified silicon nitride and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain modified silicon nitride; reacting alkali lignin with N-(P-maleimidophenyl)isocyanate and allyl isocyanate to obtain modified lignin; and mixing and vulcanizing natural rubber with the modified lignin and the modified silicon nitride to obtain the heat-stable inner tube material;
[0007] The pre-modified silicon nitride is prepared by polymerizing and growing vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol on pre-treated silicon nitride;
[0008] The pretreated silicon nitride is prepared by reacting silicon nitride and allyltriethoxysilane.
[0009] A method for preparing a heat-stable inner tube material, the method comprising the following steps:
[0010] (1) Pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:(2-3):(0.03-0.05):(30-40), and 2-amino-1,3,5-triazine-4,6-dithiol (0.7-0.8 times the molar amount of vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane) was added, and the mixture was stirred at 70-80°C and 300-500 r / min for 6-8 hours. The mixture was filtered and washed with anhydrous ethanol and deionized water respectively. Wash 3 to 5 times, dry at 50 to 60°C for 8 to 10 hours under vacuum conditions to obtain pre-modified silicon nitride; mix pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide, and acetonitrile in a mass ratio of 1:(2 to 3):(0.03 to 0.05):(10 to 12), stir at 50 to 60°C and 300 to 500 r / min for 7 to 8 hours, filter, wash with anhydrous ethanol and deionized water for 3 to 5 times each, and dry at 50 to 60°C for 8 to 10 hours under vacuum conditions to obtain modified silicon nitride;
[0011] (2) Alkali lignin, N-(P-maleimidophenyl) isocyanate, allyl isocyanate, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(0.1-0.2):(0.2-0.3):(8-10), and 0.001-0.002 times of dibutyltin dilaurate is added to the alkali lignin. The mixture is stirred at 60-70°C and 300-500 r / min for 2-3 h, and dried at 50-60°C for 7-9 h under vacuum conditions to obtain modified lignin.
[0012] (3) Dilute the natural rubber latex with water to a solid content of 30-32%. Under the conditions of 10-30°C and 300-500 r / min stirring, add a mixed modified liquid of 0.8-1 times the mass of the natural rubber latex at a uniform rate within 20 minutes, add a flocculant of 0.6-0.8 times the mass of the natural rubber latex, let it stand for 10-12 hours, filter, and dry at 50-60°C under vacuum conditions for 8-10 hours to obtain a masterbatch; mix the masterbatch, zinc oxide with a particle size of 300-500 nm, and stearic acid in a mass ratio of 1:(0.01-0.03):(0.01-0.03) and place it in a mixer. The mixture was mixed for 10-20 min at 100-120 ° C and 300-500 r / min under stirring conditions, and 0.01-0.03 times the mass of the masterbatch of 2-(4-morpholinethio)benzothiazole was added, and the mixing was continued for 10-20 min to obtain a rubber mixture, which was placed in an open mixing mill and thinned for 4-6 times at 150-160 ° C, and 0.01-0.03 times the mass of the masterbatch of sulfur with a mesh size of 400-600 was added, and the mixture was thinned for 6-8 times at 150-160 ° C, and the mixture was allowed to stand for 10-12 h. The mixture was placed on a flat vulcanizer for vulcanization for 1-2 h to obtain a heat-stable inner tube material.
[0013] As an optimization, the preparation method of the pretreated silicon nitride in step (1) is: silicon nitride and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(50~60), silane hydrolyzate is added in an amount of 8~10 times the mass of silicon nitride, the mixture is stirred at 50~60°C and 300~500r / min for 2~3h, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 50~60°C under vacuum conditions for 8~10h to obtain pretreated silicon nitride.
[0014] As an optimization, the preparation method of the silane hydrolyzate is: allyl triethoxysilane and anhydrous ethanol are mixed evenly in a mass ratio of 1: (20~30), the pH is adjusted to 4~6 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 10~30°C and 300~500r / min for 50~60min to prepare a silane hydrolyzate.
[0015] As an optimization, the particle size of the silicon nitride is 2~3μm.
[0016] As an optimization, the preparation method of the mixed modified liquid in step (3) is: uniformly mix the modified lignin, modified silicon nitride and deionized water in a mass ratio of 1:(2-3):(10-12), and ultrasonically disperse for 20-30 minutes to prepare a mixed modified liquid.
[0017] As an optimization, the flocculant in step (3) is a calcium chloride aqueous solution with a concentration of 5 mg / ml.
[0018] As an optimization, the process parameters of the vulcanization in step (3) are as follows: the temperature of the flat vulcanizing press is set to 150-160° C. and the pressure is set to 14-16 MPa.
[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0020] When preparing the heat-stable inner tube material, the present invention comprises the following steps: reacting silicon nitride and allyl triethoxysilane to obtain pretreated silicon nitride; polymerizing and growing vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol on the pretreated silicon nitride to obtain premodified silicon nitride; reacting the premodified silicon nitride and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain modified silicon nitride; reacting alkali lignin with N-(P-maleimidophenyl) isocyanate and allyl isocyanate to obtain modified lignin; and mixing and vulcanizing natural rubber, the modified lignin and the modified silicon nitride to obtain the heat-stable inner tube material.
[0021] Firstly, silicon nitride and allyltriethoxysilane are reacted to obtain pretreated silicon nitride, and a carbon-carbon double bond is introduced into the pretreated silicon nitride; vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol are polymerized and grown on the pretreated silicon nitride, and the vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane is made excessive to obtain pre-modified silicon nitride, and a triazine structure, an amino group, a Si-O bond and a fluorine atom are introduced into the pre-modified silicon nitride; the triazine structure can generate non-flammable nitrogen-containing gas, absorb heat, dilute oxygen concentration, and improve the flame retardant properties of the heat-stable inner tube material; the bond energy of the Si-O bond is greater than that of the CC bond, so compared with the CC bond, the Si-O bond needs to absorb more heat and its own vibration energy to resolve the energy of thermal decomposition of the polymer material, and the introduction of the Si-O bond can improve the thermal stability of the heat-stable inner tube material; fluorine The atoms have low reactivity and hydrophobicity, which can improve the corrosion resistance of heat-stable inner tube materials; the amino group on the pre-modified silicon nitride reacts with the PH bond on 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain modified silicon nitride, and the DOPO structure is introduced into the modified silicon nitride to further improve the flame retardant properties of the heat-stable inner tube material; because the vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane is excessive, the surface of the modified silicon nitride still retains carbon-carbon double bonds, which can participate in the vulcanization of the rubber to form a cross-linked network; silicon nitride is an inorganic material with high thermal conductivity. The compatibility of silicon nitride and rubber is improved through chemical modification, so that silicon nitride is evenly dispersed in the rubber, giving full play to the thermal conductivity of silicon nitride, improving the thermal conductivity of the heat-stable inner tube material, reducing the thermal expansion coefficient of the heat-stable inner tube material, and further improving the thermal stability of the heat-stable inner tube material.
[0022] Secondly, alkali lignin is reacted with N-(P-maleimidophenyl) isocyanate and allyl isocyanate to obtain modified lignin, and maleimide groups and carbon-carbon double bonds are introduced into the modified lignin; the carbon-carbon double bonds introduced into the modified lignin can participate in the vulcanization of the rubber to form a cross-linked network; during the thermo-oxidative aging process of the rubber, oxygen attacks the α-H on the rubber molecular chain to generate conjugated dienes; the maleimide groups introduced into the modified lignin can undergo a Diels-Alder reaction with the conjugated dienes, thereby repairing the molecular network structure destroyed by the aging process and giving the heat-stable inner tube material anti-aging properties; lignin is a natural aromatic polymer containing a large number of active phenolic hydroxyl groups, which can capture the generated free radicals during the thermo-oxidative aging process, thereby terminating the chain reaction, preventing the further development of the aging process, and further improving the anti-aging properties of the heat-stable inner tube material. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1
[0024] A method for preparing a heat-stable inner tube material, the method comprising the following steps:
[0025] (1) Allyl triethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:20, the pH was adjusted to 4 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 10°C and 300 r / min for 60 min to prepare a silane hydrolyzate; silicon nitride and anhydrous ethanol were mixed at a mass ratio of 1:50, 8 times the mass of silicon nitride was added with the silane hydrolyzate, and the mixture was stirred at 50°C and 300 r / min for 3 h, filtered, washed with anhydrous ethanol for 3 times, and dried at 50°C under vacuum for 10 h to prepare pretreated silicon nitride; pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed at a mass ratio of 1:2:0.03:30 The mixture was mixed evenly, 0.7 times the molar amount of vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane 2-amino-1,3,5-triazine-4,6-dithiol was added, the mixture was stirred at 70°C and 300 r / min for 8 hours, filtered, washed with anhydrous ethanol and deionized water 3 times each, and dried at 50°C for 10 hours under vacuum conditions to obtain pre-modified silicon nitride; the pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide, and acetonitrile were mixed evenly at a mass ratio of 1:2:0.03:10, stirred at 50°C and 300 r / min for 8 hours, filtered, washed with anhydrous ethanol and deionized water 3 times each, and dried at 50°C for 10 hours under vacuum conditions to obtain modified silicon nitride;
[0026] (2) Alkali lignin, N-(P-maleimidophenyl) isocyanate, allyl isocyanate, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.1:0.2:8, and 0.001 times of dibutyltin dilaurate was added to the alkali lignin. The mixture was stirred at 60°C and 300 r / min for 3 h, and dried at 50°C for 9 h under vacuum conditions to obtain modified lignin.
[0027] (3) The modified lignin, modified silicon nitride and deionized water were mixed in a mass ratio of 1:2:10, and ultrasonically dispersed for 20 minutes to prepare a mixed modified liquid; the natural latex was diluted with water to a solid content of 30%, and under stirring conditions of 10°C and 300 r / min, 0.8 times the mass of the natural latex of the mixed modified liquid was added at a uniform rate within 20 minutes, and 0.6 times the mass of the natural latex of a 5 mg / ml calcium chloride aqueous solution was added, and the mixture was allowed to stand for 10 hours, filtered, and dried at 50°C under vacuum conditions for 10 hours to obtain a masterbatch; the masterbatch, zinc oxide with a particle size of 300 nm, and stearic acid were added. The acid is mixed evenly in a mass ratio of 1:0.01:0.01, placed in an internal mixer, mixed for 20 minutes at 100°C and 300r / min stirring conditions, and then 0.01 times the mass of the masterbatch 2-(4-morpholinethio)benzothiazole is added, and mixing is continued for 20 minutes to obtain a rubber mixture, which is placed in an open mixer, thinned 4 times at 150°C, 0.01 times the mass of the masterbatch 400-mesh sulfur is added, thinned 6 times at 150°C, left for 10 hours, and vulcanized on a flat vulcanizer at a temperature of 150°C and a pressure of 14MPa for 2 hours to obtain a heat-stable inner tube material. Example 2
[0028] A method for preparing a heat-stable inner tube material, the method comprising the following steps:
[0029] (1) Allyl triethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:25, the pH was adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 20°C and 400 r / min for 55 min to prepare a silane hydrolyzate; silicon nitride and anhydrous ethanol were mixed at a mass ratio of 1:55, 9 times the mass of silicon nitride was added with the silane hydrolyzate, and the mixture was stirred at 55°C and 400 r / min for 2.5 h, filtered, washed with anhydrous ethanol for 4 times, and dried at 55°C under vacuum for 9 h to prepare pretreated silicon nitride; pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed at a mass ratio of 1:2.5:0.04:35 The mixture was mixed evenly, 0.75 times the molar amount of vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane 2-amino-1,3,5-triazine-4,6-dithiol was added, the mixture was stirred at 75°C and 400 r / min for 7 hours, filtered, washed with anhydrous ethanol and deionized water 4 times each, and dried at 55°C for 9 hours under vacuum conditions to obtain pre-modified silicon nitride; the pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide, and acetonitrile were mixed evenly at a mass ratio of 1:2.5:0.04:11, stirred at 55°C and 400 r / min for 7.5 hours, filtered, washed with anhydrous ethanol and deionized water 4 times each, and dried at 55°C for 9 hours under vacuum conditions to obtain modified silicon nitride;
[0030] (2) Alkali lignin, N-(P-maleimidophenyl) isocyanate, allyl isocyanate, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.15:0.25:9, and 0.0015 times of dibutyltin dilaurate was added to the alkali lignin. The mixture was stirred at 65°C and 400 r / min for 2.5 h, and dried at 55°C for 8 h under vacuum conditions to obtain modified lignin.
[0031] (3) The modified lignin, modified silicon nitride and deionized water were mixed in a mass ratio of 1:2.5:11, and ultrasonically dispersed for 25 minutes to prepare a mixed modified liquid; the natural latex was diluted with water to a solid content of 31%, and under stirring conditions of 20°C and 400 r / min, 0.9 times the mass of the natural latex of the mixed modified liquid was added at a uniform rate within 20 minutes, and 0.7 times the mass of the natural latex of a 5 mg / ml calcium chloride aqueous solution was added, and the mixture was allowed to stand for 11 hours, filtered, and dried at 55°C under vacuum conditions for 9 hours to obtain a masterbatch; the masterbatch, zinc oxide with a particle size of 400 nm, and stearic acid were added to the mixture. The acid was mixed evenly in a mass ratio of 1:0.02:0.02, placed in an internal mixer, mixed for 15 minutes at 110°C and 400r / min stirring conditions, and then 0.02 times the mass of the masterbatch 2-(4-morpholinethio)benzothiazole was added, and mixing was continued for 15 minutes to obtain a rubber mixture. The rubber mixture was placed in an open mixer, thinned 5 times at 155°C, 0.02 times the mass of the masterbatch 500-mesh sulfur was added, thinned 7 times at 155°C, parked for 11 hours, and vulcanized on a flat vulcanizer at a temperature of 155°C and a pressure of 15MPa for 1.5 hours to obtain a heat-stable inner tube material. Example 3
[0032] A method for preparing a heat-stable inner tube material, the method comprising the following steps:
[0033] (1) Allyl triethoxysilane and anhydrous ethanol were mixed at a mass ratio of 1:30, the pH was adjusted to 6 with a 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 30°C and 500 r / min for 50 min to prepare a silane hydrolyzate; silicon nitride and anhydrous ethanol were mixed at a mass ratio of 1:60, 10 times the mass of silicon nitride was added to the silane hydrolyzate, and the mixture was stirred at 60°C and 500 r / min for 2 h, filtered, washed with anhydrous ethanol for 5 times, and dried at 60°C under vacuum conditions for 8 h to prepare pretreated silicon nitride; pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed at a mass ratio of 1:3:0.05:40 The pre-modified silicon nitride was prepared by mixing the pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide and acetonitrile in a mass ratio of 1:3:0.05:12, and the mixture was stirred at 60°C and 500 r / min for 7 h. The mixture was filtered, washed with anhydrous ethanol and deionized water for 5 times, and dried at 60°C for 8 h under vacuum to obtain the pre-modified silicon nitride. The pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide and acetonitrile were mixed in a mass ratio of 1:3:0.05:12, and the mixture was stirred at 60°C and 500 r / min for 7 h. The mixture was filtered, washed with anhydrous ethanol and deionized water for 5 times, and dried at 60°C for 8 h under vacuum to obtain the modified silicon nitride.
[0034] (2) Alkali lignin, N-(P-maleimidophenyl) isocyanate, allyl isocyanate, and N,N-dimethylformamide were mixed evenly in a mass ratio of 1:0.2:0.3:10, and 0.002 times of dibutyltin dilaurate was added to the alkali lignin. The mixture was stirred at 70°C and 500 r / min for 2 h, and dried at 60°C for 7 h under vacuum conditions to obtain modified lignin.
[0035] (3) The modified lignin, modified silicon nitride and deionized water were mixed in a mass ratio of 1:3:12, and ultrasonically dispersed for 30 minutes to prepare a mixed modified liquid; the natural latex was diluted with water to a solid content of 32%, and under stirring conditions of 30°C and 500 r / min, the mixed modified liquid with a mass of 1 times the mass of the natural latex was added at a uniform rate within 20 minutes, and a calcium chloride aqueous solution with a concentration of 5 mg / ml with a mass of 0.8 times the mass of the natural latex was added, and the mixture was allowed to stand for 10 hours, filtered, and dried at 60°C under vacuum conditions for 8 hours to obtain a masterbatch; the masterbatch, zinc oxide with a particle size of 500 nm, and stearic acid were added. The mixture was mixed evenly in a mass ratio of 1:0.03:0.03, placed in an internal mixer, mixed for 10 minutes at 120°C and 500r / min stirring conditions, and then 0.03 times the mass of the masterbatch of 2-(4-morpholinethio)benzothiazole was added, and mixing was continued for 10 minutes to obtain a rubber mixture, which was placed in an open mixer, thinned 4 times at 160°C, 0.03 times the mass of the mixture of 600 mesh sulfur was added, thinned 6 times at 160°C, allowed to stand for 12 hours, and vulcanized on a flat vulcanizer at a temperature of 160°C and a pressure of 16MPa for 1 hour to obtain a heat-stable inner tube material.
[0036] Comparative Example 1
[0037] The difference between the preparation method of the heat-stable inner tube material of Comparative Example 1 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: allyl triethoxysilane and anhydrous ethanol are mixed evenly at a mass ratio of 1:25, the pH value is adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 20°C and 400 r / min for 55 min to prepare a silane hydrolyzate; silicon nitride and anhydrous ethanol are mixed evenly at a mass ratio of 1:55, silane hydrolyzate with a mass of 9 times that of silicon nitride is added, the mixture is stirred at 55°C and 400 r / min for 2.5 h, filtered, washed with anhydrous ethanol 4 times, and dried at 55°C under vacuum for 9 h to prepare modified silicon nitride. The remaining steps are the same as those of Example 2.
[0038] Comparative Example 2
[0039] The preparation method of the heat-stable inner tube material of Comparative Example 2 is different from that of Example 2 in that step (1) is different. Step (1) is modified as follows: allyl triethoxysilane and anhydrous ethanol are mixed uniformly in a mass ratio of 1:25, the pH value is adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 20°C and 400 r / min for 55 min to prepare a silane hydrolyzate; silicon nitride and anhydrous ethanol are mixed uniformly in a mass ratio of 1:55, silane hydrolyzate with 9 times the mass of silicon nitride is added, the mixture is stirred at 55°C and 400 r / min for 2.5 h, filtered, washed 4 times with anhydrous ethanol, and dried under vacuum at 55°C. ℃ and dried for 9 hours to obtain pretreated silicon nitride; pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:2.5:0.04:35, and 2-amino-1,3,5-triazine-4,6-dithiol with a molar amount of 0.75 times of vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane was added, stirred at 75℃ and 400r / min for 7 hours, filtered, washed with anhydrous ethanol and deionized water 4 times each, and dried at 55℃ for 9 hours under vacuum conditions to obtain modified silicon nitride. The remaining steps are the same as those in Example 2.
[0040] Comparative Example 3
[0041] The preparation method of the heat-stable inner tube material of Comparative Example 3 is different from that of Example 2 in that step (1) is not performed, and step (3) is modified as follows: the modified lignin, silicon nitride, and deionized water are uniformly mixed in a mass ratio of 1:2.5:11, and ultrasonically dispersed for 25 minutes to prepare a mixed modified liquid; the natural latex is diluted with water to a solid content of 31%, and under stirring conditions of 20°C and 400 r / min, 0.9 times the mass of the natural latex of the mixed modified liquid is uniformly added within 20 minutes, and 0.7 times the mass of the natural latex and a concentration of 5 mg / ml of calcium chloride aqueous solution is added, and the mixture is allowed to stand for 11 hours, filtered, and dried at 55°C under vacuum conditions for 9 hours to obtain a masterbatch. ; The masterbatch, zinc oxide with a particle size of 400nm, and stearic acid are mixed uniformly in a mass ratio of 1:0.02:0.02, placed in an internal mixer, mixed for 15min at 110℃ and 400r / min stirring conditions, then 0.02 times the mass of the masterbatch of 2-(4-morpholinethio)benzothiazole are added, and the mixing is continued for 15min to obtain a rubber mix, the rubber mix is placed in an open mixer, thinned 5 times at 155℃, 0.02 times the mass of the rubber mix of 500 mesh sulfur is added, thinned 7 times at 155℃, parked for 11h, and vulcanized on a flat vulcanizer at a temperature of 155℃ and a pressure of 15MPa for 1.5h to obtain a heat-stable inner tube material. The remaining steps are the same as in Example 2.
[0042] Comparative Example 4
[0043] The preparation method of the heat-stable inner tube material of Comparative Example 4 is different from that of Example 2 in that step (2) is not performed, and step (3) is modified as follows: alkali lignin, modified silicon nitride, and deionized water are uniformly mixed in a mass ratio of 1:2.5:11, and ultrasonically dispersed for 25 minutes to prepare a mixed modified liquid; natural latex is diluted with water to a solid content of 31%, and under stirring conditions of 20°C and 400r / min, 0.9 times the mass of the natural latex of the mixed modified liquid is uniformly added within 20 minutes, and 0.7 times the mass of the natural latex and a concentration of 5mg / ml of calcium chloride aqueous solution is added, and the mixture is allowed to stand for 11 hours, filtered, and dried at 55°C under vacuum conditions for 9 hours to obtain a mother tube. Rubber; Masterbatch, zinc oxide with a particle size of 400nm, and stearic acid are mixed uniformly in a mass ratio of 1:0.02:0.02, placed in an internal mixer, mixed for 15min at 110℃ and 400r / min stirring conditions, then 0.02 times the mass of the masterbatch of 2-(4-morpholinethio)benzothiazole is added, and mixing is continued for 15min to obtain a mixed rubber, the mixed rubber is placed in an open mixer, thinned 5 times at 155℃, 0.02 times the mass of the mixed rubber of 500 mesh sulfur is added, thinned 7 times at 155℃, parked for 11h, and vulcanized on a flat vulcanizer at a temperature of 155℃ and a pressure of 15MPa for 1.5h to obtain a heat-stable inner tube material. The remaining steps are the same as in Example 2.
[0044] Test Example 1
[0045] Flame retardant performance test
[0046] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T2406.2, and the limiting oxygen index of the standard specimens was tested. The results are shown in Table 1.
[0047] Table 1
[0048]
[0049] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 1, it can be found that the heat-stable inner tube material prepared by the present invention has good flame retardant properties.
[0050] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Examples 1 to 3, indicating that the pretreated silicon nitride is prepared by reacting silicon nitride and allyltriethoxysilane, and a carbon-carbon double bond is introduced into the pretreated silicon nitride; vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol are polymerized and grown on the pretreated silicon nitride, and the vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane is allowed to form a pretreated silicon nitride. The method comprises the following steps: preparing a pre-modified silicon nitride by adding an excess of alkyl, and introducing a triazine structure and an amino group into the pre-modified silicon nitride; the triazine structure can generate a non-flammable nitrogen-containing gas, absorb heat, dilute the oxygen concentration, and improve the flame retardant properties of the heat-stable inner tube material; the amino group on the pre-modified silicon nitride is reacted with the PH bond on 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to prepare a modified silicon nitride, and introducing a DOPO structure into the modified silicon nitride to further improve the flame retardant properties of the heat-stable inner tube material.
[0051] Test Example 2
[0052] Corrosion resistance test
[0053] Test method: The water drop contact angle of the embodiment and the comparative example was tested using the sessile drop method on an OCA20 contact angle meter, and the water drop volume was 5 μL. The results are shown in Table 2
[0054] Table 2
[0055]
[0056] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 2, it can be found that the heat-stable inner tube material prepared by the present invention has good corrosion resistance.
[0057] By comparison, the contact angles of Examples 1 to 3 are greater than those of Comparative Examples 1 and 3, indicating that pretreated silicon nitride is obtained by reacting silicon nitride and allyltriethoxysilane, and carbon-carbon double bonds are introduced into the pretreated silicon nitride; vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol are polymerized and grown on the pretreated silicon nitride, and vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane is made excessive to obtain pre-modified silicon nitride, and fluorine atoms are introduced into the pre-modified silicon nitride; fluorine atoms have low reactivity and hydrophobicity, and can improve the corrosion resistance of the thermally stable inner tube material.
[0058] Test Example 3
[0059] Anti-aging performance test
[0060] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T1040, and their tensile strength was tested. The examples and comparative examples were treated at a temperature of 50°C and an oxygen concentration of 32% under normal pressure for 36 hours, and their tensile strength was tested. The change rate of the tensile strength of the examples and comparative examples before and after the thermal oxidative aging treatment was calculated. The results are shown in Table 3.
[0061] Table 3
[0062]
[0063] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 3, it can be found that the heat-stable inner tube material prepared by the present invention has good anti-aging performance.
[0064] By comparison, the change rate of tensile strength of Examples 1 to 3 is less than that of Comparative Example 4, indicating that the modified lignin is obtained by reacting alkali lignin with N-(P-maleimidophenyl)isocyanate and allyl isocyanate, and maleimide groups and carbon-carbon double bonds are introduced into the modified lignin; the carbon-carbon double bonds introduced into the modified lignin can participate in the vulcanization of the rubber to form a cross-linked network; during the thermal oxidative aging of the rubber, oxygen attacks the α-H on the rubber molecular chain to generate conjugated dienes; the maleimide groups introduced into the modified lignin can undergo a Diels-Alder reaction with the conjugated dienes, thereby repairing the molecular network structure destroyed by the aging process, and giving the heat-stable inner tube material anti-aging properties.
[0065] Test Example 4
[0066] Thermal stability test
[0067] Test method: The examples and comparative examples were prepared into standard specimens according to GB / T1040, and their tensile strength was tested at room temperature and then at 120°C, and the change rate of the tensile strength of the examples and comparative examples after heat treatment was calculated. The results are shown in Table 4.
[0068] Table 4
[0069]
[0070] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 4 in Table 4, it can be found that the heat-stable inner tube material prepared by the present invention has good heat stability.
[0071] By comparison, the change rates of tensile strength of Examples 1 to 3 are less than those of Comparative Examples 1 and 3, indicating that pretreated silicon nitride is prepared by reacting silicon nitride and allyltriethoxysilane, and a carbon-carbon double bond is introduced into the pretreated silicon nitride; vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane and 2-amino-1,3,5-triazine-4,6-dithiol are polymerized and grown on the pretreated silicon nitride, and vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane is made excessive to prepare pre-modified silicon nitride, and Si-O bonds are introduced into the pre-modified silicon nitride; Si- The bond energy of the O bond is greater than that of the CC bond, so compared with the CC bond, the Si-O bond needs to absorb more heat and its own vibration energy to dissipate the energy of thermal decomposition of the polymer material. The introduction of the Si-O bond can improve the thermal stability of the thermally stable inner tube material; silicon nitride is an inorganic material with high thermal conductivity. The compatibility of silicon nitride and rubber is improved through chemical modification, so that silicon nitride is evenly dispersed in the rubber, and the thermal conductivity of silicon nitride is fully utilized, thereby improving the thermal conductivity of the thermally stable inner tube material, reducing the thermal expansion coefficient of the thermally stable inner tube material, and further improving the thermal stability of the thermally stable inner tube material.
[0072] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a heat-stable inner tube material, characterized in that: The preparation method of the thermally stable inner tube material comprises the following preparation steps: (1) Pretreated silicon nitride, vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane, azobisisobutyronitrile, and N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:(2-3):(0.03-0.05):(30-40), 2-amino-1,3,5-triazine-4,6-dithiol (0.7-0.8 times the molar amount of vinyl-terminated dimethylmethyl-3,3,3-trifluoropropylsiloxane) was added, and the mixture was stirred at 70-80°C and 300-500 r / min for 6-8 hours, filtered, washed with anhydrous ethanol and deionized water for 3-5 times each, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain pre-modified silicon nitride; Pre-modified silicon nitride, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, cuprous iodide and acetonitrile are uniformly mixed in a mass ratio of 1:(2-3):(0.03-0.05):(10-12), stirred at 50-60°C and 300-500 r / min for 7-8 hours, filtered, washed with anhydrous ethanol and deionized water for 3-5 times respectively, and dried at 50-60°C under vacuum conditions for 8-10 hours to obtain modified silicon nitride; (2) Alkali lignin, N-(P-maleimidophenyl) isocyanate, allyl isocyanate, and N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(0.1-0.2):(0.2-0.3):(8-10), and 0.001-0.002 times of dibutyltin dilaurate is added to the alkali lignin. The mixture is stirred at 60-70°C and 300-500 r / min for 2-3 h, and dried at 50-60°C for 7-9 h under vacuum conditions to obtain modified lignin. (3) Dilute the natural rubber latex with water to a solid content of 30-32%. Under the conditions of 10-30°C and 300-500 r / min stirring, add a mixed modified liquid of 0.8-1 times the mass of the natural rubber latex at a uniform rate within 20 minutes, add a flocculant of 0.6-0.8 times the mass of the natural rubber latex, let it stand for 10-12 hours, filter, and dry at 50-60°C under vacuum conditions for 8-10 hours to obtain a masterbatch; mix the masterbatch, zinc oxide with a particle size of 300-500 nm, and stearic acid in a mass ratio of 1:(0.01-0.03):(0.01-0.03) and place it in a mixer. The mixture was mixed for 10 to 20 minutes at 100 to 120°C and 300 to 500 r / min under stirring conditions, and then 0.01 to 0.03 times the mass of the masterbatch of 2-(4-morpholinethio)benzothiazole was added, and the mixing was continued for 10 to 20 minutes to obtain a rubber mixture, and the rubber mixture was placed in an open mixer, and thinned 4 to 6 times at 150 to 160°C, and 0.01 to 0.03 times the mass of the rubber mixture of 400 to 600 mesh sulfur was added, and thinned 6 to 8 times at 150 to 160°C, and the mixture was parked for 10 to 12 hours, and the mixture was placed on a flat vulcanizer for vulcanization for 1 to 2 hours to obtain a heat-stable inner tube material; The preparation method of the pretreated silicon nitride in step (1) is as follows: silicon nitride and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(50-60), silane hydrolyzate is added in an amount of 8-10 times the mass of silicon nitride, the mixture is stirred at 50-60°C and 300-500 r / min for 2-3 hours, filtered, washed with anhydrous ethanol for 3-5 times, and dried at 50-60°C under vacuum for 8-10 hours to obtain pretreated silicon nitride; The preparation method of the silane hydrolyzate is as follows: allyl triethoxysilane and anhydrous ethanol are uniformly mixed in a mass ratio of 1:(20-30), the pH value is adjusted to 4-6 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 10-30° C. and 300-500 r / min for 50-60 min to prepare the silane hydrolyzate; The preparation method of the mixed modified liquid in step (3) is as follows: the modified lignin, the modified silicon nitride and the deionized water are uniformly mixed in a mass ratio of 1:(2-3):(10-12), and ultrasonically dispersed for 20-30 minutes to prepare a mixed modified liquid.
2. The method for preparing a heat-stable inner tube material according to claim 1, characterized in that: The particle size of the silicon nitride is 2-3 μm.
3. The method for preparing a heat-stable inner tube material according to claim 1, characterized in that: The flocculant in step (3) is a calcium chloride aqueous solution with a concentration of 5 mg / ml.
4. The method for preparing a heat-stable inner tube material according to claim 1, characterized in that: The process parameters of the vulcanization in step (3) are as follows: the temperature of the flat vulcanizing press is set to 150-160° C. and the pressure is set to 14-16 MPa.
5. A heat-stable inner tube material prepared according to the method for preparing a heat-stable inner tube material according to any one of claims 1 to 4.