Environment-friendly water-based art repair coating as well as preparation and application thereof

By using raw materials such as modified silica and nano-titanium dioxide in water-based coatings, the antibacterial performance of the coating is improved, which solves the problem of insufficient antibacterial performance of existing water-based coatings in medical and food places, and achieves efficient antibacterial and antibacterial properties. Mold effect.

CN118755291APending Publication Date: 2024-10-11SICHUAN TONGSHEN WATERPROOF ENG CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410888851.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing water-based coatings have insufficient antibacterial performance in special places such as medical and food, making it difficult to meet high safety and environmental standards.

Method used

Powder and liquid are mixed at a ratio of 3.5mL:1g. The powder includes cement, talcum powder, modified silica, nano-titanium dioxide and cellulose. The porosity and zinc oxide of the coating are improved through the preparation method of modified silica. Crystal formation, combined with the photocatalytic performance of nano-titanium dioxide, enhances the antibacterial effect.

Benefits of technology

The environmentally friendly water-based paint prepared has an antibacterial rate of 99.98% and a level 0 antifungal performance, which is significantly higher than existing paints and meets the antibacterial needs of special places.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004926850180000081
    Figure BDA0004926850180000081
  • Figure BDA0004926850180000091
    Figure BDA0004926850180000091
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses an environment-friendly water-based art repair coating as well as preparation and application thereof. The invention relates to an environment-friendly water-based art repair coating, which is prepared by mixing a powder material and a liquid material according to a mass volume ratio of 3.5 mL: 1g. The powder material comprises the following raw materials in parts by mass: 40-60 parts of cement, 20-40 parts of talcum powder, 10-20 parts of modified white carbon black, 1-3 parts of nano titanium dioxide and 1-10 parts of cellulose; the liquid material is prepared from the following raw materials in parts by volume: 30 to 50 parts of water, 1 to 5 parts of water-soluble polyurethane, 0.2 to 0.5 part of preservative and 0.5 to 1.5 parts of defoaming agent. The prepared environment-friendly water-based art repair coating has good antibacterial performance, and the antibacterial rate can reach 99.98% and is far higher than that of an existing antibacterial coating; the environment-friendly water-based art repair coating prepared by the preparation method disclosed by the invention has good anti-mildew performance, and the mildew growing grade reaches 0 grade which is superior to that of the existing coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, and in particular to an environmentally friendly water-based art repair paint and a preparation method and application thereof. Background Art

[0002] Water-based paint is a type of paint that uses water as a solvent. Compared to traditional oil-based paint, the solvent of water-based paint contains only a small amount of alcohol ether organic solvents, which greatly reduces the content of harmful substances in the paint and improves the safety and environmental protection of the paint.

[0003] However, with the continuous improvement of people's quality of life, the requirements for building decoration materials are also gradually increasing. Simple environmental protection and safety can no longer fully meet the construction needs of some special places, especially in medical and food places, which put forward higher requirements on the antibacterial properties of coatings; therefore, preparing a water-based coating that is both safe and environmentally friendly and has good antibacterial effect has become a technical problem that technicians in this field urgently need to solve. Summary of the invention

[0004] The purpose of the present invention is to provide an environmentally friendly water-based art repair paint, which is safe and environmentally friendly and has a good antibacterial effect, and can meet the antibacterial requirements of special places such as medical and food.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] One of the technical solutions of the present invention:

[0007] An environmentally friendly water-based art repair paint is prepared by mixing powder and liquid in a mass volume ratio of 3.5 mL:1 g.

[0008] Furthermore, the powder comprises the following raw materials in parts by weight: 40 to 60 parts of cement, 20 to 40 parts of talc, 10 to 20 parts of modified white carbon black, 1 to 3 parts of nano titanium dioxide and 1 to 10 parts of cellulose;

[0009] Preferably, the powder comprises the following raw materials in parts by weight: 50 parts of cement, 30 parts of talcum powder, 15 parts of modified white carbon black, 2 parts of nano titanium dioxide and 5 parts of cellulose.

[0010] The present invention uses talcum powder as a raw material, which has good dispersibility. Therefore, when it is applied to a coating, it can be evenly and stably dispersed in the coating, thereby avoiding the problems of precipitation and stratification of the coating during use. In addition, the talcum powder also has good hygroscopicity, which can absorb excess moisture in the coating, thereby preventing the problems of flowing and deformation caused by excessive moisture in the coating. Moreover, the good hygroscopicity of the talcum powder can also reduce the agglomeration of white carbon black, carbon fiber, nano titanium dioxide and cellulose, thereby avoiding the problem that the raw materials cannot effectively function due to agglomeration, thereby effectively improving the antibacterial performance of the coating.

[0011] Furthermore, the preparation method of the modified silica comprises the following steps: etching the silica in an alkaline solvent, then immersing the silica in a zinc ammonia solution, and performing microwave crystallization to obtain zinc oxide-silica, namely the modified silica.

[0012] Furthermore, the alkaline solvent is a 0.5 mol / L sodium hydroxide solution;

[0013] Furthermore, the mass volume ratio of the white carbon black to the alkaline solvent is 1 g:10 mL;

[0014] Furthermore, the etching is performed at 50 to 70° C. for 20 to 40 minutes;

[0015] Preferably, the etching is performed at 60° C. for 30 minutes.

[0016] The present invention uses white carbon black as a raw material, which can effectively improve the weather resistance of the coating; research has found that although talcum powder has good dispersibility and hygroscopicity, its weather resistance is poor. In order to compensate for the weather resistance of talcum powder, the present invention adds white carbon black to the raw materials; in addition, some other raw materials such as silica ash also have good weather resistance, but the reason why the present invention does not select other raw materials is that other raw materials cannot form effective zinc oxide crystals and have poor adsorption to zinc oxide crystals, thereby reducing the antibacterial performance of the coating.

[0017] The present invention performs alkali solvent heating etching modification on white carbon black, which can effectively improve the porosity of white carbon black and the specific surface area of ​​white carbon black, thereby providing space for the subsequent formation of as many zinc oxide crystals as possible, thereby improving the antibacterial performance of the finally prepared coating; the present invention can more effectively improve the porosity and ensure the effective formation of zinc oxide crystals by controlling the etching temperature; research has found that if the etching temperature is too low, the etching effect is not obvious, and a high porosity cannot be achieved, resulting in fewer zinc oxide crystals and reducing the antibacterial performance of the coating; if the etching temperature is too high, the porosity is large, and zinc oxide crystals are formed during subsequent washing. Crystals will fall off due to washing, thereby reducing the number of zinc oxide crystals and causing the coating to have a decreased antibacterial performance. Moreover, excessively high temperatures will also destroy the microporous structure of silica, making it impossible to retain zinc oxide crystals, making the coating lack antibacterial properties. In addition, silica has poor dispersibility, and if it is directly impregnated with zinc ammonia solution, it will not be evenly dispersed, resulting in agglomeration. However, after it is modified with an alkaline reagent, a certain amount of cations and anions will remain on its surface. The presence of these anions and cations can improve the dispersibility of silica to a certain extent, thereby better achieving the formation of zinc oxide crystals.

[0018] Furthermore, the immersion treatment is specifically as follows: placing the white carbon black after the alkali etching treatment in a zinc ammonia solution, adding hexadecyltrimethylammonium bromide, and immersing the solution with the assistance of ultrasonic wave;

[0019] Furthermore, the preparation method of the zinc ammonia solution is: controlling the stirring speed to 40 rpm, placing analytical pure ammonia water in analytical pure zinc hydroxide according to the mass volume ratio of analytical pure zinc hydroxide to analytical pure ammonia water of 1 g:5 mL to form a turbid liquid, then maintaining the stirring speed at 40 rpm, adding analytical pure ammonia water dropwise to the turbid liquid until no zinc hydroxide precipitates and the solution is translucent, filtering with suction, and diluting the filtrate with water to obtain a zinc ammonia solution with a concentration of 900 ppm;

[0020] Furthermore, the mass volume ratio of the white carbon black, the zinc ammonia solution and the hexadecyltrimethylammonium bromide is 1 g:25 mL:0.05 g;

[0021] Furthermore, in the ultrasonic-assisted immersion treatment, the wavelength of the ultrasonic wave is 15 mm and the treatment time is 5 to 15 min;

[0022] Preferably, the ultrasonic-assisted immersion treatment lasts for 10 minutes.

[0023] The present invention crystallizes nano zinc oxide in the micropores of white carbon black, which can effectively improve the antibacterial performance of the coating; the nano zinc oxide can generate photogenerated holes under light conditions, which can convert oxygen in the environment into activated oxygen. The extremely strong oxidizing activity of the activated oxygen can be used to oxidize and kill bacteria and other microorganisms in the environment. In addition, zinc ions in the zinc oxide can be freed. When the zinc ions come into contact with bacteria, the protease in the bacteria will be deformed and inactivated, thereby killing the bacteria.

[0024] The present invention adopts microwave-assisted impregnation and adds a certain amount of hexadecyltrimethylammonium bromide, which can make the zinc ammonia solution penetrate into the micropores of white carbon black better, thereby increasing the content of nano zinc oxide crystals and achieving better antibacterial performance of the coating; in addition, the present invention limits the wavelength and treatment time of ultrasound, which can better achieve the penetration of the zinc ammonia solution. Experiments show that increasing or decreasing the wavelength and increasing or decreasing the treatment time will lead to reduced antibacterial performance. After analysis, the reason is that the increase in wavelength and the decrease in time will lead to the incomplete penetration of the zinc ammonia solution, thereby resulting in less zinc oxide crystals and reducing the antibacterial performance of the coating, while the reduction in wavelength and the increase in treatment time will cause the microporous structure of white carbon black to be destroyed. Although more zinc oxide crystals can be formed, the adhesion is not strong. The zinc oxide crystals will fall off after washing with water, thereby reducing the antibacterial performance of the coating.

[0025] The invention adopts a zinc ammonia solution with a relatively low concentration, which can improve the stability of the zinc ammonia solution in an ultrasonic environment while ensuring the content of zinc oxide crystals; the zinc ammonia solution is substantially a solution formed by zinc ammonia complex ions, and the increase in temperature (ultrasonic treatment will inevitably cause thermal effects) will cause the zinc ammonia complex ions to dissociate into zinc ions and ammonium ions (the complex ions are unstable, and changes in external conditions can cause them to dissociate into simple ions), thereby failing to achieve the formation of zinc oxide crystals; the zinc ammonia solution with a relatively low concentration, that is, a relatively high water content, can quickly disperse heat when ultrasound generates a thermal effect, thereby reducing the temperature and increasing the possibility of destroying the zinc ammonia complex ions; in addition, when the concentration of the zinc ammonia solution is too low, the amount of zinc ammonia complex ions that penetrate into the interior of white carbon black is too small, thereby causing a reduction in the content of zinc oxide crystals.

[0026] Furthermore, the microwave crystallization is specifically as follows: treating the impregnated silica with microwaves for 1 to 10 minutes, and then placing the microwave-treated silica in water for crystallization at 150°C;

[0027] Furthermore, the microwave frequency of the microwave treatment is 915 MHz, and the crystallization time is 2 to 4 hours;

[0028] Preferably, the microwave treatment time is 5 min and the crystallization time is 3 h;

[0029] Furthermore, after microwave crystallization, the silica needs to be washed with water until no zinc oxide crystals exist on the surface of the silica.

[0030] The present invention utilizes microwave treatment to promote the formation of nano zinc oxide crystal nuclei and reduce the crystal formation time. If microwave treatment is not used, the crystal formation time will be slow, and when the micropore surface is smooth, there is a situation where fewer crystals are formed or even no crystals can be formed, thereby causing the antibacterial rate of the coating to decrease. In addition, microwave treatment can form relatively dispersed nano zinc oxide crystal nuclei inside the white carbon black micropores, thereby improving the antibacterial performance of the coating. If microwave treatment is omitted, the crystals can only grow freely, which is not conducive to the dispersion of the crystals, resulting in poor antibacterial effect of the coating.

[0031] The present invention selects microwaves with a frequency of 915, which has a poor heating efficiency and can reduce the damage to white carbon black and zinc oxide crystals, and has a certain protective effect on white carbon black and zinc oxide crystals. The reason for not selecting microwaves with a lower frequency is that the frequency of 915 is a lower frequency of common industrial microwave frequencies, which is a choice made in consideration of economic factors. In addition, the experimental results in the laboratory research stage show that although the reduction of microwave frequency can reduce the damage to white carbon black and zinc oxide crystals, the volume of the formed crystal nuclei is small, and some micropores cannot effectively form crystal nuclei, which is not conducive to the formation of zinc oxide crystals, thereby resulting in a decrease in antibacterial performance.

[0032] The present invention uses nano titanium dioxide as a raw material and can effectively improve the antibacterial effect of the coating; analysis shows that nano titanium dioxide has unique photocatalytic properties. Under the excitation of light, nano titanium dioxide can produce free radicals with strong oxidizing properties, and these free radicals can destroy the cell structure of bacteria, thereby achieving the purpose of antibacterial; in addition, experimental results show that nano titanium dioxide and nano zinc oxide have a synergistic effect, and the reason may be that the interaction between the two can expand the excitation wavelength range and improve the efficiency of the photocatalytic reaction.

[0033] Furthermore, the cellulose is hydroxypropyl methylcellulose.

[0034] Furthermore, the liquid material comprises the following raw materials by volume: 30 to 50 parts of water, 1 to 5 parts of water-soluble polyurethane, 0.2 to 0.5 parts of preservative and 0.5 to 1.5 parts of defoaming agent;

[0035] Preferably, the liquid material comprises the following raw materials in parts by volume: 40 parts of water, 2 parts of water-soluble polyurethane, 0.3 parts of preservative and 0.7 parts of defoaming agent.

[0036] The present invention adds water-soluble polyurethane as a water-soluble resin in the coating, which can effectively improve the weather resistance and acid and alkali resistance of the coating and improve the mechanical properties of the coating.

[0037] The second technical solution of the present invention:

[0038] The preparation method of the above-mentioned environmentally friendly water-based art repair paint comprises the following steps:

[0039] Weigh the raw materials according to the mass or volume parts, mix cement, talcum powder, modified white carbon black, nano titanium dioxide and cellulose to obtain powder, mix water, water-soluble polyurethane, preservative and defoamer to obtain liquid, and finally mix the powder and liquid to obtain the environmentally friendly water-based art repair paint.

[0040] The third technical solution of the present invention:

[0041] The above-mentioned environmentally friendly water-based art paint is used in substrate painting.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1) The water-based art paint prepared by the present invention has good antibacterial performance, and the antibacterial rate can reach 99.98%, which is much higher than the existing antibacterial paint;

[0044] 2) The water-based art paint prepared by the present invention has good anti-fungal performance, and the mold growth level reaches level 0, which is better than the existing paint. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] Unless otherwise specified, the "parts" described in the present invention are measured by mass or volume according to the state of the raw materials; in the following examples, the raw materials are weighed according to 1 part = 1 g or 1 part = 1 mL.

[0047] In the following examples, an environmentally friendly water-based art paint is prepared by mixing a powder and a liquid in a mass volume ratio of 3.5 mL:1 g.

[0048] The powder comprises the following raw materials by weight: 40 to 60 parts of cement, 20 to 40 parts of talc, 10 to 20 parts of modified white carbon black, 1 to 3 parts of nano titanium dioxide and 1 to 10 parts of cellulose;

[0049] The preparation method of the modified white carbon black comprises the following steps:

[0050] 1) mixing white carbon black with 0.5 mol / L sodium hydroxide solution at a mass volume ratio of 1 g:10 mL, and etching at 60° C. for 30 min to obtain alkaline-etched white carbon black;

[0051] 2) controlling the stirring speed to 40 rpm, placing analytically pure ammonia water in analytically pure zinc hydroxide according to a mass volume ratio of analytically pure zinc hydroxide to analytically pure ammonia water of 1 g:5 mL to form a turbid solution, then maintaining the stirring speed at 40 rpm, dropwise adding analytically pure ammonia water into the turbid solution until no zinc hydroxide precipitates and the solution becomes translucent, filtering with suction, and diluting the filtrate with water to obtain a zinc ammonia solution with a concentration of 900 ppm;

[0052] 3) placing the alkaline-etched white carbon black obtained in step 1) in the zinc ammonia solution obtained in step 2), and adding hexadecyltrimethylammonium bromide, mixing and stirring for 1 minute, wherein the mass volume ratio of white carbon black, zinc ammonia solution and hexadecyltrimethylammonium bromide is 1g:25mL:0.05g, then controlling the ultrasonic wavelength to 15mm, and immersing for 10 minutes;

[0053] 4) treating the silica after the immersion treatment in step 3) with a microwave at a frequency of 915 MHz for 5 min, then placing the silica in water, controlling the ambient temperature to 150° C., and crystallizing for 3 h, and finally washing the silica with water until no zinc oxide crystals are present on the surface, thereby obtaining zinc oxide-silica, i.e., modified silica;

[0054] The cellulose is hydroxypropyl methylcellulose;

[0055] The liquid material comprises the following raw materials by volume: 30-50 parts of water, 1-5 parts of water-soluble polyurethane, 0.2-0.5 parts of preservative and 0.5-1.5 parts of defoaming agent.

[0056] In the following embodiments, a method for preparing an environmentally friendly water-based art paint comprises the following steps:

[0057] Weigh the raw materials according to the mass or volume parts, mix cement, talcum powder, modified white carbon black, nano titanium dioxide and cellulose to obtain powder, mix water, water-soluble polyurethane, preservative and defoamer to obtain liquid, and finally mix the powder and liquid to obtain the environmentally friendly water-based art repair paint.

[0058] In the following embodiments, the cement is PO42.5 ordinary Portland cement purchased from Wuxi Jianghuai Building Materials Technology Co., Ltd.; the talc is 1250 mesh talc purchased from Lingshou County Zhan Teng Mineral Products; the white carbon black is A200 fumed white carbon black purchased from Delan Chemical; the nano titanium dioxide is anatase nano titanium dioxide purchased from Nanjing Baoket New Materials Co., Ltd.; the hydroxypropyl methylcellulose is purchased from Renqiu Shangxiang Environmental Protection Materials Factory; the water-soluble polyurethane is a water-based polyurethane resin purchased from Hefei Huayue New Materials Technology Co., Ltd.; the preservative is a Kathon preservative purchased from Jinan Zhongbei Fine Chemical Co., Ltd.; the defoamer is a water-based paint defoamer purchased from Guangdong Nanhui New Materials.

[0059] Example 1

[0060] An environmentally friendly water-based art paint

[0061] 1) Weigh each raw material according to the mass parts or volume parts recorded in 1# in Table 1;

[0062] 2) mixing the white carbon black weighed in step 1) with 0.5 mol / L sodium hydroxide solution at a mass volume ratio of 1 g:10 mL, and etching at 60° C. for 30 min to obtain alkaline-etched white carbon black;

[0063] 3) controlling the stirring speed to 40 rpm, placing analytically pure ammonia water in analytically pure zinc hydroxide according to a mass volume ratio of analytically pure zinc hydroxide to analytically pure ammonia water of 1 g:5 mL to form a turbid solution, then maintaining the stirring speed at 40 rpm, dropwise adding analytically pure ammonia water into the turbid solution until no zinc hydroxide precipitates and the solution becomes translucent, filtering with suction, and diluting the filtrate with water to obtain a zinc ammonia solution with a concentration of 900 ppm;

[0064] 4) placing the alkaline-etched white carbon black obtained in step 2) in the zinc ammonia solution obtained in step 3), and adding hexadecyltrimethylammonium bromide, mixing and stirring for 1 minute, wherein the mass volume ratio of white carbon black, zinc ammonia solution and hexadecyltrimethylammonium bromide is 1g:25mL:0.05g, then controlling the ultrasonic wavelength to 15mm, and immersing for 10 minutes;

[0065] 5) treating the silica after the immersion treatment in step 4) with a microwave at a frequency of 915 MHz for 5 min, then placing the silica in water, controlling the ambient temperature to 150° C., and crystallizing for 3 h, and finally washing the silica with water until no zinc oxide crystals are present on the surface, thereby obtaining zinc oxide-silica, i.e., modified silica;

[0066] 6) mixing the cement, talcum powder, nano titanium dioxide and hydroxypropyl methylcellulose weighed in step 1) and the modified silica obtained in step 5), and stirring for 10 minutes to obtain a powder;

[0067] 7) Mix the water, water-soluble polyurethane, preservative and defoamer weighed in step 1) and stir for 30 minutes to obtain a liquid material;

[0068] 8) The powder obtained in step 6) and the liquid obtained in step 7) were mixed at a mass volume ratio of 3.5 mL:1 g, and stirred for 40 min to obtain an environmentally friendly water-based art repair coating.

[0069] Example 2

[0070] An environmentally friendly water-based art paint

[0071] The same as Example 1, except that step 1) is to weigh each raw material according to the mass parts or volume parts recorded in 2# in Table 1.

[0072] Example 3

[0073] An environmentally friendly water-based art paint

[0074] Same as Example 1, except that step 1) is to weigh each raw material according to the mass parts or volume parts recorded in 3# in Table 1.

[0075] Table 1 Raw material composition (parts)

[0076]

[0077]

[0078] Comparative Example 1

[0079] A water-based art paint

[0080] Same as Example 1, except that silica fume is used instead of white carbon black.

[0081] Comparative Example 2

[0082] A water-based art paint

[0083] Same as Example 1, except that step 2) is omitted.

[0084] Comparative Example 3

[0085] A water-based art paint

[0086] Same as Example 1, except that in step 2), white carbon black is etched at 40° C. for 30 min.

[0087] Comparative Example 4

[0088] A water-based art paint

[0089] Same as Example 1, except that in step 2), white carbon black is etched at 80° C. for 30 min.

[0090] Comparative Example 5

[0091] A water-based art paint

[0092] Same as Example 1, except that in step 3), the zinc ammonia solution is diluted to 1500 ppm.

[0093] Comparative Example 6

[0094] A water-based art paint

[0095] Same as Example 1, except that in step 3), the zinc ammonia solution is diluted to 500 ppm.

[0096] Comparative Example 7

[0097] A water-based art paint

[0098] The same as Example 1, the only difference is that in step 4), the ultrasonic wave length is controlled to be 30 mm, and the time of ultrasonic wave-assisted immersion treatment is controlled to be 3 min.

[0099] Comparative Example 8

[0100] A water-based art paint

[0101] The same as Example 1, except that in step 4), the ultrasonic wave length is controlled to be 10 mm, and the time of ultrasonic wave-assisted immersion treatment is controlled to be 20 min.

[0102] Comparative Example 9

[0103] A water-based art paint

[0104] The same as Example 1, except that step 5) is to place the silica after the immersion treatment in step 4) in water, control the ambient temperature to 150° C., and crystallize for 10 hours, then wash the silica with water until there is no zinc oxide crystal on the surface, to obtain zinc oxide-silica, i.e., modified silica.

[0105] Comparative Example 10

[0106] A water-based art paint

[0107] Same as Example 1, except that the frequency of the microwave treatment in step 5) is 500 MHz.

[0108] Comparative Example 11

[0109] A water-based art paint

[0110] Same as Example 1, except that the frequency of the microwave treatment in step 5) is 2000 MHz.

[0111] Comparative Example 12

[0112] A water-based art paint

[0113] The same as Example 1, the only difference is that the addition of nano titanium dioxide is omitted in step 6).

[0114] Comparative Example 13

[0115] A water-based art paint

[0116] The same as Example 1, the only difference is that nano silver ions are used instead of nano dioxide in step 6).

[0117] Effect verification

[0118] The water-based art paints prepared in Examples 1 to 3 and Comparative Examples 1 to 13 were tested for antibacterial and antifungal properties according to the testing method described in the industry standard HG / T 3950-2007. The test results are shown in Table 2:

[0119] In addition, a control example is provided, namely, an antibacterial coating commonly used in the art (Gordon water-based antibacterial glaze paint).

[0120] Table 2 Performance test

[0121] Antibacterial rate / % Mildew Grade / Level Comparison Example 99.38 1 Example 1 99.98 0 Example 2 99.97 0 Example 3 99.98 0 Comparative Example 1 - 2 Comparative Example 2 95.34 2 Comparative Example 3 97.55 1 Comparative Example 4 97.38 1 Comparative Example 5 98.96 1 Comparative Example 6 98.65 1 Comparative Example 7 97.19 2 Comparative Example 8 97.65 2 Comparative Example 9 97.95 1 Comparative Example 10 98.69 1 Comparative Example 11 95.92 2 Comparative Example 12 94.38 2 Comparative Example 13 99.83 1

[0122] Note: The antibacterial rate of “-” indicates that it has no antibacterial properties.

[0123] From the data in Table 2, it can be found that the water-based art repair paint prepared by the present invention has good antibacterial performance (the detected bacteria are: Aspergillus niger, Aspergillus terreus, Penicillium variotii, Penicillium funiculum, Aureobasidium short-stalked and Chaetomium globosum), and the antibacterial rate can reach 99.98%, which is much higher than the existing antibacterial paint (Gordon water-based antibacterial glaze paint has good performance in inhibiting Escherichia coli and Staphylococcus aureus, but for some other bacteria, such as Aspergillus niger, Aspergillus terreus, etc., the antibacterial effect is poor). Moreover, the water-based art repair paint prepared by the present invention also has good anti-mold performance, and the mold growth level reaches 0, which is better than the existing paint;

[0124] From Comparative Example 1, it can be found that the addition of white carbon black is more conducive to the formation of nano zinc oxide crystals, while replacing it with other raw materials makes it difficult for zinc oxide crystals to form, which is not conducive to the antibacterial performance of the coating;

[0125] It can be seen from Comparative Examples 2 to 4 that omitting the alkaline solvent heating etching or changing the etching temperature will have an adverse effect on the antibacterial properties of the coating;

[0126] It can be seen from Comparative Examples 5 to 6 that the concentration of the zinc-ammonia solution will affect the antibacterial performance of the coating, and the optimal antibacterial performance can only be achieved at a certain concentration;

[0127] It can be seen from Comparative Examples 7 to 8 that during ultrasonic assisted extraction, the wavelength of the ultrasonic wave and the extraction time will affect the antibacterial performance of the coating. Only by reasonably selecting the wavelength and the extraction time can the optimal antibacterial performance be achieved.

[0128] It can be seen from Comparative Examples 9 to 11 that omitting microwave crystallization or adjusting the microwave crystallization time will affect the antibacterial properties of the coating to a certain extent;

[0129] It can be seen from Comparative Examples 12 to 13 that nano-titanium dioxide and nano-zinc oxide have a synergistic effect. Omitting nano-titanium dioxide or replacing nano-titanium dioxide with other antibacterial materials will reduce the antibacterial performance of the coating.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. An environmentally friendly water-based art paint, characterized in that: The powder and liquid were mixed in a mass volume ratio of 3.5 mL:1 g.

2. The environmentally friendly water-based art paint according to claim 1, characterized in that: The powder comprises the following raw materials in parts by weight: 40 to 60 parts of cement, 20 to 40 parts of talcum powder, 10 to 20 parts of modified white carbon black, 1 to 3 parts of nano titanium dioxide and 1 to 10 parts of cellulose.

3. The environmentally friendly water-based art paint according to claim 2, characterized in that: The preparation method of the modified white carbon black comprises the following steps: etching the white carbon black in an alkaline solvent, then immersing the white carbon black in a zinc ammonia solution, and performing microwave crystallization to obtain zinc oxide-white carbon black, namely the modified white carbon black.

4. The environmentally friendly water-based art paint according to claim 3, characterized in that: The etching is performed at 50-70° C. for 20-40 minutes.

5. The environmentally friendly water-based art paint according to claim 3, characterized in that: The immersion treatment specifically includes placing the white carbon black after alkali etching treatment in a zinc ammonia solution, adding hexadecyltrimethylammonium bromide, and performing ultrasonic-assisted immersion treatment.

6. The environmentally friendly water-based art paint according to claim 3, characterized in that: The microwave crystallization specifically comprises: subjecting the impregnated silica to microwave treatment for 1 to 10 minutes, and then placing the microwave-treated silica in water to crystallize at 150°C.

7. The environmentally friendly water-based art paint according to claim 1, characterized in that: The liquid material comprises the following raw materials in parts by volume: 30-50 parts of water, 1-5 parts of water-soluble polyurethane, 0.2-0.5 parts of preservative and 0.5-1.5 parts of defoaming agent.

8. The environmentally friendly water-based art paint according to claim 1, characterized in that: The cellulose is hydroxypropyl methylcellulose.

9. A method for preparing an environmentally friendly water-based art paint as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: Weigh the raw materials according to the mass or volume parts, mix cement, talcum powder, modified white carbon black, nano titanium dioxide and cellulose to obtain powder, mix water, water-soluble polyurethane, preservative and defoamer to obtain liquid, and finally mix the powder and liquid to obtain the environmentally friendly water-based art repair paint.

10. Use of the environmentally friendly water-based art paint as claimed in any one of claims 1 to 8 in substrate painting.

Citation Information

Patent Citations

  • Environment-friendly polymer cement waterproof coating and preparation method thereof

    CN111073496A

  • Two-component waterborne polyurethane mortar waterproof coating and preparation method thereof

    CN113511855A

  • Ct inspection

    KR102549748B1