A mechanochromic film containing dithiol and its preparation method

By grafting dithiol compounds onto liquid crystals and using polythiol silsesquioxanes, the mechanical properties and color rendering effects of traditional liquid crystal coatings in mechanochromic films have been solved, improving the mechanical strength and color rendering effect of the films and expanding their application range.

CN118755293BActive Publication Date: 2024-11-12NANTONG NKODA POLYURETHANE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411238062.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Traditional liquid crystal coatings suffer from low mechanical properties, easy tearing of the surface, and poor color development when used to produce mechanochromic films. Furthermore, the small molecule initiators introduced during the photocuring process are mobile, affecting the color development, thermal stability, and viscosity of the film.

Method used

A modified liquid crystal composite was formed by pre-grafting dithiol compounds with liquid crystals to form a grafted structure, combined with polythiol silsesquioxane as a filler, and optimized by pre-composite photoinitiator and photocuring process to prepare a mechanochromic film.

Benefits of technology

It improves the mechanical strength and color development effect of the mesticolor film, reduces curing stress, enhances the thermal stability and durability of the film, and expands its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present invention relates to the technical field of mechanochromic films, specifically to a mechanochromic film containing dithiol and a preparation method thereof. Step 1: Mix a double-ended acrylic ester liquid crystal and a dithiol compound, add a thermal initiator, and react for 1.5 to 2.5 hours at a temperature of 60 to 65°C and a pressure of 1±0.1 atm to obtain a modified liquid crystal; Step 2: Add the modified liquid crystal, monoacrylate, glycidyl methacrylate, chiral dopant, polythiol silsesquioxane, and photoinitiator to a solvent in sequence to obtain a coating with a solid content of 20 to 22 wt%; Step 3: Evenly coat the coating on the surface of the base film, dry at 100 to 120°C; photocuring; and obtain a mechanochromic film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mechanochromic films, in particular to a mechanochromic film containing dithiol and a preparation method thereof. Background Art

[0002] Liquid crystal is a substance between solid and liquid with unique optical and electrical properties. It is widely used in various display devices, optical devices and sensors. Among them, mechanochromic film is a special liquid crystal material that changes color when subjected to external force, thereby achieving visual detection of force. However, traditional liquid crystal coatings have problems such as low mechanical properties, easy surface tearing, and poor color rendering when making mechanochromic films.

[0003] In the prior art, the mechanical strength and color rendering effect of liquid crystals are mainly enhanced by changing the molecular structure of liquid crystals and adding nanoparticles or other polymer materials. Although the prior art has made certain progress, there are still some problems and shortcomings, such as: (1) There are dispersion and compatibility problems in the process of introducing fillers, which have a negative impact on the optical and electrical properties of liquid crystals; (2) There is a large curing stress in the photocured mechanochromic film, which leads to high film brittleness and easy tearing on the surface; and photocuring requires the introduction of initiators. Due to the small molecular weight of common initiators, they often have migration, which affects the color rendering, thermal stability, viscosity and other properties of the film, affecting its application in real devices and sensors.

[0004] In summary, solving the above problems and preparing a mechanochromic film containing dithiol has important application value. Summary of the invention

[0005] The object of the present invention is to provide a mechanochromic film containing dithiol and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing a dithiol-containing mechanochromic film comprises the following steps:

[0008] Step 1: Mix a double-terminal acrylic ester liquid crystal and a dithiol compound, add a thermal initiator, and react at a temperature of 60-65° C. and a pressure of 1±0.1 atm for 1.5-2.5 hours to obtain a modified liquid crystal;

[0009] Step 2: adding modified liquid crystal, monoacrylate, glycidyl methacrylate, chiral dopant, polythiol silsesquioxane, and photoinitiator to a solvent in sequence to obtain a coating having a solid content of 20-22 wt %;

[0010] Step 3: evenly apply the coating on the surface of the base film, dry at 100-120°C, and light cure to obtain a mechanochromic film.

[0011] In a further embodiment, the mass ratio of the double-ended acrylic ester liquid crystal to the dithiol compound is 1:0.1.

[0012] In a further embodiment, the preparation method of the dithiol compound is: under a nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:(2~2.1) are mixed; the reaction is stirred at a temperature of 50~60°C for 4~6 hours; and the dithiol compound is purified to obtain the dithiol compound.

[0013] In a further embodiment, the coating includes the following raw materials in parts by mass: 66 to 69 parts of modified liquid crystal, 20 to 22 parts of monoacrylate, 2 to 3 parts of glycidyl methacrylate, 3 to 4 parts of chiral dopant, 2.5 to 3 parts of polythiol silsesquioxane, and 3 to 3.5 parts of photoinitiator.

[0014] In a further embodiment, the modified liquid crystal is pre-compounded with a photoinitiator to obtain a liquid crystal composite before preparing a coating; the preparation method of the liquid crystal composite is as follows: under a nitrogen atmosphere, diisocyanate and an organic tin catalyst are sequentially added to ethyl acetate, a photoinitiator is added dropwise, and the reaction is stirred at a temperature of 60-65°C for 2-3 hours; the modified liquid crystal is added, the temperature is raised to 70-80°C, the reaction is continued for 3-4 hours, and the solvent is evaporated to obtain a liquid crystal composite.

[0015] In a further embodiment, the mass ratio of the diisocyanate to the photoinitiator is 1.2-1.4:1.

[0016] In a further embodiment, the preparation method of the polythiol silsesquioxane is as follows: (1) adding polyepoxy cage silsesquioxane and lithium chloride to anhydrous tetrahydrofuran in sequence and stirring evenly, adding carbon disulfide dropwise, stirring and reacting at room temperature for 10 to 16 hours; evaporating the solvent to obtain modified silsesquioxane; (2) adding modified silsesquioxane and ethylamine to anhydrous tetrahydrofuran, stirring at room temperature for 12 to 24 hours, evaporating the solvent to obtain polythiol silsesquioxane.

[0017] In a further embodiment, in the modified silsesquioxane, the mass ratio of polyepoxy cage silsesquioxane, lithium chloride and carbon disulfide is 10:0.5~0.6:15~18; in the polythiol silsesquioxane, the mass ratio of modified silsesquioxane and ethylamine is 1:4~5.

[0018] In a further embodiment, the photocuring process conditions are: 50-100 mW / cm 2 Light cure under ultraviolet light for 5 to 10 minutes.

[0019] In a further embodiment, a method for preparing a dithiol-containing mechanochromic film provides a mechanochromic film.

[0020] Compared with the prior art, the present application has the following beneficial effects:

[0021] In the (1) scheme, a dithiol compound is used to pre-bond the liquid crystal to form a grafted structure. Compared with directly dispersing the two substances in the coating and directly curing them, pre-grafting can increase the viscosity of the liquid crystal and reduce the curing stress of direct curing, thereby solving the problem of easy tearing of the surface of traditional liquid crystal coatings when making mechanochromic films.

[0022] At the same time, dithiol compounds are used to graft and modify the liquid crystal instead of grafting to change the molecular structure of the liquid crystal. Therefore, this modification method has little effect on the optical and electrical properties of the liquid crystal and will not limit the application of the device in real devices and sensors.

[0023] (2) By adjusting and limiting the type and amount of dithiol compounds, the color rendering effect of liquid crystal is optimized so that it can show brighter and more lasting colors when subjected to external force, thereby solving the problem of poor color rendering effect and improving the accuracy and sensitivity of visual force detection.

[0024] Among them, the dithiol compound is based on 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane, and first utilizes the ring-opening reaction of the amino group in mercaptoethylamine and its epoxy group to graft mercapto groups at both ends to obtain the dithiol compound. Among them, the silicon oxygen chain contained is an electrically auxiliary color group, which can enhance the color change effect; at the same time, it can improve the thermal stability of the film; and it can produce stress buffering during the curing process, thereby improving the mechanical properties and tear resistance of the film, thereby expanding the application range of the mechanochromic film. However, the introduction of this chain segment should not be too high, which will interfere with the normal arrangement of liquid crystal molecules and reduce the color development effect. Therefore, the mass ratio of the double-ended acrylic ester liquid crystal to the dithiol compound is limited in the scheme.

[0025] (3) Compared with the common method of directly introducing small molecule photoinitiators, in this scheme, the small molecule initiator is pre-grafted onto the modified liquid crystal using diisocyanate to obtain a liquid crystal composite; the small molecule mobility is effectively solved, the dispersibility of the photoinitiator is increased, the uniformity and rate of photocuring are improved, the concentrated stress is reduced, the quality of the mechanochromic film is improved, and the durability and service life of the mechanochromic film are improved.

[0026] (4) In the scheme, polythiol silsesquioxane is further introduced as a filler. The tetrathiol group in the polythiol silsesquioxane increases the cross-linking property, thereby increasing the adhesion strength. At the same time, the silsesquioxane has a colloidally connected silicon-oxygen skeleton, which can effectively enhance the thermal stability and mechanical properties. The cage-type framework gives it good optical properties. Its introduction can effectively enhance toughness, buffer photocuring stress, reduce stress accumulation, further improve the performance of the mechanochromic film, improve the efficiency and sensitivity of the mechanochromic film, and expand the application range of the mechanochromic film in the fields of force visualization detection, pressure sensing, and stress analysis. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are exemplified without any special restrictions: in the following embodiments, parts are parts by mass; the double-ended acrylic ester liquid crystal C3M is 1,4-bis[4-(3-acryloxypropoxy)benzoyloxy]-2-methylbenzene; the acrylic monomer RM105 is 4-methoxyphenyl 4-((6-(acryloxy)hexyl)oxy)benzoate; the chiral dopant is chiral agent R5011, the brand is Bayi Liquid Crystal; the CAS number of polyepoxy cage-type silsesquioxane is 307496-38-4, all of which are commercially available.

[0029] Example 1: A method for preparing a mechanochromic film containing dithiol, comprising the following steps:

[0030] Pre-preparation: (1) Under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:2.1 were mixed; the mixture was stirred at 50°C for 6 hours; and the mixture was purified to obtain a dithiol compound; (2) 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride were added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide were added dropwise, and the mixture was stirred at room temperature for 12 hours; the solvent was evaporated to obtain a modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine were added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent was evaporated to obtain a polythiol silsesquioxane;

[0031] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0032] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3.2 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 67 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0033] (2) Liquid crystal composite, 20 parts of monoacrylate (acrylic monomer RM105, 2-ethylhexyl acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, 4 parts of chiral agent R5011, and 2.8 parts of polythiol silsesquioxane were sequentially added into a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0034] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0035] Example 2: A method for preparing a mechanochromic film containing dithiol, comprising the following steps:

[0036] Pre-preparation: (1) Under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:2.1 were mixed; the mixture was stirred at 50°C for 6 hours; and the mixture was purified to obtain a dithiol compound; (2) 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride were added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide were added dropwise, and the mixture was stirred at room temperature for 12 hours; the solvent was evaporated to obtain a modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine were added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent was evaporated to obtain a polythiol silsesquioxane;

[0037] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0038] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 66 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0039] (2) Liquid crystal composite, 22 parts of monoacrylate (acrylic monomer RM105, 2-ethylhexyl acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, 3 parts of chiral agent R5011, and 3 parts of polythiol silsesquioxane were sequentially added to a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0040] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0041] Example 3: A method for preparing a dithiol-containing mechanochromic film, comprising the following steps:

[0042] Pre-preparation: (1) Under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:2.1 were mixed; the mixture was stirred at 50°C for 6 hours; and the mixture was purified to obtain a dithiol compound; (2) 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride were added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide were added dropwise, and the mixture was stirred at room temperature for 12 hours; the solvent was evaporated to obtain a modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine were added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent was evaporated to obtain a polythiol silsesquioxane;

[0043] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0044] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3.5 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 69 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0045] (2) The liquid crystal composite, 20 parts of monoacrylate (acrylic acid monomer RM105 and (2-ethylhexyl) acrylate in a mass ratio of 7:1), 2 parts of glycidyl methacrylate, 3 parts of chiral agent R5011, and 2.5 parts of polythiol silsesquioxane were sequentially added into a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0046] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0047] Comparative Example 1: Referring to Example 1, the modified liquid crystal and the photoinitiator are not pre-compounded, and a method for preparing a mechanochromic film containing dithiol comprises the following steps:

[0048] Pre-preparation: (1) Under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:2.1 were mixed; the mixture was stirred at 50°C for 6 hours; and the mixture was purified to obtain a dithiol compound; (2) 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride were added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide were added dropwise, and the mixture was stirred at room temperature for 12 hours; the solvent was evaporated to obtain a modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine were added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent was evaporated to obtain a polythiol silsesquioxane;

[0049] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0050] Step 2: 67 parts of modified liquid crystal, 20 parts of monoacrylate (acrylic monomer RM105, 2-ethylhexyl acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, 4 parts of chiral agent R5011, 3.2 parts of photoinitiator 1173, and 2.8 parts of polythiol silsesquioxane were sequentially added into a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20wt%;

[0051] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0052] Comparative Example 2: Referring to Example 1, the amount of dithiol compound introduced was increased; a method for preparing a mechanochromic film containing dithiol, comprising the following steps:

[0053] Pre-preparation: (1) Under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:2.1 were mixed; the mixture was stirred at 50°C for 6 hours; and the mixture was purified to obtain a dithiol compound; (2) 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride were added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide were added dropwise, and the mixture was stirred at room temperature for 12 hours; the solvent was evaporated to obtain a modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine were added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent was evaporated to obtain a polythiol silsesquioxane;

[0054] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.2, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0055] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3.2 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 67 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0056] (2) Liquid crystal composite, 20 parts of monoacrylate (acrylic monomer RM105, 2-ethylhexyl acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, 4 parts of chiral agent R5011, and 2.8 parts of polythiol silsesquioxane were sequentially added into a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0057] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0058] Comparative Example 3: Referring to Example 1, the dithiol compound is replaced with 2,2-(1,2-ethylenedioxy)bis(ethyl mercaptan), and a method for preparing a mechanochromic film containing dithiol comprises the following steps:

[0059] Pre-preparation: 10 parts of polyepoxy cage-type silsesquioxane and 0.5 parts of lithium chloride are added to 100 parts of anhydrous tetrahydrofuran in sequence and stirred evenly, 18 parts of carbon disulfide are added dropwise, and the mixture is stirred and reacted at room temperature for 12 hours; the solvent is evaporated to obtain modified silsesquioxane; 10 parts of modified silsesquioxane and 45 parts of ethylamine are added to 200 parts of anhydrous tetrahydrofuran, stirred at room temperature for 24 hours, and the solvent is evaporated to obtain polythiol silsesquioxane;

[0060] Step 1: Mix double-terminal acrylic ester liquid crystal C3M and 2,2-(1,2-ethylenedioxy)bis(ethyl mercaptan) in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60°C and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0061] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3.2 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 67 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0062] (2) Liquid crystal composite, 20 parts of monoacrylate (acrylic monomer RM105, 2-ethylhexyl acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, 4 parts of chiral agent R5011, and 2.8 parts of polythiol silsesquioxane were sequentially added into a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0063] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0064] Comparative Example 4, referring to Example 1, without introducing polythiol silsesquioxane, a method for preparing a dithiol-containing mechanochromic film comprises the following steps:

[0065] Preparative preparation: (1) under nitrogen atmosphere, 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine were mixed in a molar ratio of 1:2.1; stirred and reacted at 50° C. for 6 hours; purified to obtain a dithiol compound;

[0066] Step 1: Mix a double-terminal acrylic ester liquid crystal C3M and a dithiol compound in a mass ratio of 1:0.1, add azobisisobutyronitrile, and react at a temperature of 60° C. and a pressure of 1 atm for 2 hours to obtain a modified liquid crystal;

[0067] Step 2: (1) Under a nitrogen atmosphere, diisophorone diisocyanate (accounting for 1.2 times the mass of the photoinitiator) and dibutyltin dilaurate are added to ethyl acetate in sequence, 3.2 parts of the photoinitiator 1173 are added dropwise, and the mixture is stirred and reacted at 60°C for 2 hours; 67.8 parts of the modified liquid crystal are added, the temperature is raised to 75°C, and the reaction is continued for 4 hours, and the solvent is evaporated to obtain a liquid crystal composite;

[0068] (2) The liquid crystal composite, 22 parts of monoacrylate (acrylic acid monomer RM105 and (2-ethylhexyl) acrylate in a mass ratio of 7:1), 3 parts of glycidyl methacrylate, and 4 parts of chiral agent R5011 were sequentially added to a solvent (cyclohexanone and ethyl acetate in a volume ratio of 4:1) to obtain a coating with a solid content of 20 wt%;

[0069] Step 3: Apply the coating evenly on the surface of the base film, dry at 120°C to remove the solvent; 2 The film was cured under UV light for 6 minutes to obtain a mechanochromic film.

[0070] Performance Test 1: The mechanochromic film in Example 1 was subjected to a stretching color change experiment to observe the color change; the obtained data are shown in the following table:

[0071]

[0072] Conclusion: The initial elongation of the mechanochromic film is 100%. As the elongation changes, the color changes from red to different colors through different elongations, and the colors are red, orange, yellow, green, cyan, blue and purple respectively.

[0073] Performance Test 2: The mechanochromic films prepared in the examples and comparative examples were subjected to a tensile test at a rate of 3 mm / min to obtain the relationship between stress and tensile length; and the tensile force corresponding to the maximum blue shift; the obtained data are shown in the following table:

[0074]

[0075] Conclusion: From the data in the above table, it can be seen that the process of pre-compounding modified liquid crystal and photoinitiator, regulating the amount of dithiol compounds introduced, limiting disulfide compounds containing siloxanes, and introducing thiol silsesquioxanes all effectively enhance the quality of the mechanochromic film; through the limitation of these characteristics in the application, the problem of easy surface tearing and color sensitivity of traditional liquid crystal coatings in the production of mechanochromic films is effectively solved, and a mechanochromic film with good mechanics and high stress sensitivity is prepared, which improves the durability and service life of the mechanochromic film.

[0076] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a mechanochromic film containing dithiol, characterized in that: The following steps are involved: Step 1: Mix a double-terminal acrylic ester liquid crystal and a dithiol compound, add a thermal initiator, and react at a temperature of 60-65° C. and a pressure of 1±0.1 atm for 1.5-2.5 hours to obtain a modified liquid crystal; Step 2: (1) Under a nitrogen atmosphere, add diisocyanate and organotin catalyst to ethyl acetate in sequence, add photoinitiator dropwise, and stir to react at a temperature of 60-65°C for 2-3 hours; add modified liquid crystal, raise the temperature to 70-80°C and continue to react for 3-4 hours, and evaporate the solvent to obtain a liquid crystal composite; (2) Add the liquid crystal composite, monoacrylate, methacrylate glycidyl ether, chiral dopant, and polythiol silsesquioxane to the solvent in sequence to obtain a coating with a solid content of 20-22wt%; Step 3: uniformly apply the coating on the surface of the base film, dry at 100-120°C, and light-cure to obtain a mechanochromic film; The mass ratio of the double-terminal acrylic ester liquid crystal to the dithiol compound is 1:0.1; The preparation method of the dithiol compound comprises: mixing 1,3-bis(3-glycidyloxypropyl)-1,1,3,3-tetramethyldisiloxane and mercaptoethylamine in a molar ratio of 1:(2-2.1) under a nitrogen atmosphere; stirring and reacting at a temperature of 50-60° C. for 4-6 hours; and purifying to obtain the dithiol compound; The preparation method of the polythiol silsesquioxane is as follows: (1) adding polyepoxy cage-type silsesquioxane and lithium chloride to anhydrous tetrahydrofuran in sequence and stirring evenly, adding carbon disulfide dropwise, stirring and reacting at room temperature for 10 to 16 hours; evaporating the solvent to obtain modified silsesquioxane; (2) adding modified silsesquioxane and ethylamine to anhydrous tetrahydrofuran, stirring at room temperature for 12 to 24 hours, evaporating the solvent to obtain polythiol silsesquioxane.

2. The method for preparing a dithiol-containing mechanochromic film according to claim 1, characterized in that: The coating comprises the following raw materials in parts by weight: 66-69 parts of modified liquid crystal, 20-22 parts of monoacrylate, 2-3 parts of glycidyl methacrylate, 3-4 parts of chiral dopant, 2.5-3 parts of polythiol silsesquioxane, and 3-3.5 parts of photoinitiator.

3. The method for preparing a dithiol-containing mechanochromic film according to claim 1, characterized in that: The mass ratio of the diisocyanate to the photoinitiator is 1.2-1.4:

1.

4. The method for preparing a dithiol-containing mechanochromic film according to claim 1, characterized in that: In the modified silsesquioxane, the mass ratio of polyepoxy cage silsesquioxane, lithium chloride and carbon disulfide is 10:0.5-0.6:15-18; in the polythiol silsesquioxane, the mass ratio of modified silsesquioxane and ethylamine is 1:4-5.

5. The method for preparing a dithiol-containing mechanochromic film according to claim 1, characterized in that: The process conditions of the light curing are: 50~100mW / cm 2 Light cure under ultraviolet light for 5 to 10 minutes. 6 . The mechanochromic film prepared by the method for preparing a mechanochromic film containing dithiol according to claim 1 .