Radiation-proof coating
By hydrolyzing methyltrimethoxysilane in acrylic emulsion to form silica sol, and combining nano CeO2 and graphene oxide, the polymerization of silica gel is directly completed, which solves the complex preparation process and low thermal insulation performance of existing thermal insulation coatings. problem, achieving coatings with high thermal insulation and mechanical properties and simplifying the production process.
Patent Information
- Application Number
- CN202410929539.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-11
AI Technical Summary
The preparation process of existing thermal insulation coatings is complex. It is difficult to mix the silica aerogel evenly in acrylic acid, resulting in a reduction in thermal insulation performance, and the surface modifier affects the coating structure.
Methyltrimethoxysilane is hydrolyzed in acrylic emulsion to form silica sol. The polymerization of silica gel is directly completed in acrylic emulsion to form a conjugated three-dimensional network structure. Combined with nano-CeO2 and graphene oxide, it simplifies the production steps and improves Thermal insulation and mechanical properties.
It significantly improves the thermal insulation and mechanical properties of the coating, reduces the thermal conductivity, enhances the stability and durability of the coating, simplifies the production process and reduces the cost.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a radiation protection coating. Background Art
[0002] Energy conservation and carbon reduction is one of the key measures to address climate change and environmental protection challenges, aiming to achieve sustainable development and reduce the impact on the earth's climate system. In the field of construction, thermal insulation materials are usually used to reduce energy loss in buildings to achieve the purpose of energy conservation and emission reduction. Thermal insulation coatings can reduce heat conduction by reflecting, absorbing or blocking heat, thereby effectively reducing heat absorption and loss of buildings or equipment.
[0003] Silica aerogel is a high-performance porous material, known for its extremely low thermal conductivity, high porosity and large specific surface area. In the prior art, as disclosed in the document with Chinese patent publication number CN108610815A, a thermal insulation coating is prepared from raw materials including silica aerogel, titanium dioxide, hollow glass microspheres, and far-infrared ceramic powder, wherein the mass ratio of silica aerogel, titanium dioxide, hollow glass microspheres and far-infrared ceramic powder is 2-7:3-8:3-8:6-16; the thermal insulation coating is prepared by the following steps: grinding silica aerogel particles into powder, adding a wetting agent, a dispersant, and 1 / 3-1 / 2 a defoaming agent to deionized water, and stirring at a speed of 300-500r / min. After stirring for 3 to 5 minutes, add silica aerogel powder, increase the speed to 1800 to 2000 r / min, and make it high-speed shear dispersion for 2 to 3 hours to prepare silica aerogel slurry, then reduce the speed to 600 to 800 r / min, add acrylic resin and film-forming aid, stir evenly, finally add titanium dioxide, far-infrared ceramic powder, hollow glass microbeads and the remaining defoaming agent in turn, mix evenly to obtain silica aerogel composite thermal insulation coating; use a wire rod coater to evenly apply the coating on the aluminum alloy plate, the coating wet film thickness is 120 to 150 μm, and dry under natural conditions to obtain.
[0004] However, in the above preparation steps, silica aerogel particles need to be prepared in advance, the preparation process is complicated, and since silica aerogel is difficult to mix evenly in acrylic acid, it requires long-term mechanical mixing or surface modification, and the surface modifier can easily change the structure of the coating and reduce the thermal insulation performance of the coating. Summary of the invention
[0005] In order to solve the problems in the above-mentioned background technology, the first object of the present invention is to provide an anti-radiation coating, which has low thermal conductivity and excellent thermal insulation and mechanical properties.
[0006] The solution adopted by the present invention to solve the technical problem is:
[0007] A radiation protection coating comprises the following raw materials in parts: 50-70 parts of acrylic emulsion, 2-5 parts of ammonia water, 15-20 parts of acetic acid, 10-20 parts of water, 30-45 parts of methyltrimethoxysilane, 2-5 parts of graphene oxide, 1-7 parts of nano CeO2, 1.5-3 parts of surfactant, 2-3 parts of defoaming agent and 2.5-5.5 parts of dispersant.
[0008] The second object of the present invention is to provide a method for producing a radiation-proof coating with a simple process and stable product performance.
[0009] S1: acetic acid, a surfactant, and methyltrimethoxysilane were mixed together and stirred for 10 min to obtain a mixture 1;
[0010] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0011] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0012] S4: Pour polyvinyl alcohol, water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 200-300 r / min for 10-15 min until the diameter of the nano-CeO2 is 20nm-25nm;
[0013] S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add water and stir at a speed of 300-400 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0014] The present application directly completes the polymerization of silica gel in acrylic emulsion, thereby simplifying the production steps and reducing costs.
[0015] Silane forms a conjugated three-dimensional network structure in the coating, which improves the thermal insulation performance of the coating. The conjugated three-dimensional network structure of silane and the evaporation of water in the process of drying and shrinking of the coating make a large number of nano-scale pores on the coating. The air trapped in these pores can reduce the conduction heat, thereby significantly improving the thermal insulation capacity of the thermal insulation coating.
[0016] The gel particles are partially embedded in the acrylic matrix, resulting in a large number of pores on the cross-section of the acrylic matrix. The increase in the number of pores further reduces the thermal conductivity of the coating and improves the thermal insulation performance of the coating. At the same time, the acrylic matrix also strengthens the skeleton of the silane, which helps to resist pore collapse caused by capillary forces and retain pores during the drying process.
[0017] Silane is synthesized in the coating, and silica is connected by chemical bonds to form a complete heterogel network inside the coating, so that the silica heterogel particles are evenly dispersed in the coating without agglomeration. At the same time, the mechanical properties of the thermal insulation coating are improved.
[0018] In summary, the beneficial effects of the present invention are:
[0019] Methyltrimethoxysilane is hydrolyzed with acetic acid to obtain silica sol, which forms silica isogel in acrylic emulsion. The silanol groups in the silica sol can form hydrogen bonds and covalent bonds with the oxygen-containing functional groups on the surface of graphene oxide. The two-dimensional layered graphene oxide and silica isogel can form a stable multilayer structure, which improves the thermal insulation and mechanical properties of the coating.
[0020] Nano-CeO2 has a high specific surface area and porosity. The ground nano-CeO2 can be filled in the paint and evenly dispersed in the paint, increasing the thermal resistance of the paint, reducing heat transfer, and improving the stability of the paint at high temperatures. In addition, the combined effect of graphene oxide and nano-CeO2 also improves the durability of the paint.
[0021] Polyvinyl alcohol and sodium bicarbonate are helpful to disperse nano-CeO2 uniformly.
[0022] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following preferred embodiments are specifically cited and described in detail as follows. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Embodiment 1
[0025] A radiation-proof coating, comprising the following raw materials by weight: silicon dioxide, 50 parts of acrylic emulsion, 2 parts of ammonia water, 15 parts of acetic acid, 10 parts of water, 30 parts of methyltrimethoxysilane, 2 parts of graphene oxide, 1 part of nano CeO2, 1 part of polyvinyl pyrrolidone, 2 parts of isopropanol, 5 parts of polyvinyl alcohol, and 0.5 parts of sodium bicarbonate;
[0026] The following steps are involved:
[0027] S1: acetic acid, polyvinyl pyrrolidone and methyltrimethoxysilane were mixed together and stirred for 10 min to obtain a mixture 1;
[0028] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0029] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0030] S4: Pour polyvinyl alcohol, 2 parts of water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 200 r / min for 10 min until the diameter of the nano-CeO2 is 25 nm;
[0031] S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add 8 parts of water, stir at 300 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0032] Embodiment 2
[0033] A radiation-proof coating, comprising the following raw materials by weight: 60 parts of acrylic emulsion, 3 parts of ammonia water, 17 parts of acetic acid, 20 parts of water, 35 parts of methyltrimethoxysilane, 2 parts of graphene oxide, 7 parts of nano CeO2, 6.5 parts of polyvinyl alcohol, 2.5 parts of isopropanol, and 0.5 parts of sodium bicarbonate;
[0034] The following steps are involved:
[0035] S1: acetic acid, 1.5 parts of polyvinyl alcohol and methyltrimethoxysilane were mixed together and stirred for 10 minutes to obtain a mixture 1;
[0036] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0037] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0038] S4: Pour 5 parts of polyvinyl alcohol, 2 parts of water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 200 r / min for 10 minutes until the diameter of the nano-CeO2 is 24 nm;
[0039] S5: Pour the defoamer and the ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add 18 parts of water, stir at a speed of 300 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0040] Embodiment 3
[0041] A radiation-proof coating, comprising the following raw materials by weight: 70 parts of acrylic emulsion, 2 parts of ammonia water, 20 parts of acetic acid, 18 parts of water, 45 parts of methyltrimethoxysilane, 5 parts of graphene oxide, 1 part of nano CeO2, 2 parts of ethanol, 5 parts of polyvinyl alcohol, and 0.5 parts of sodium bicarbonate;
[0042] The following steps are involved:
[0043] S1: Mix acetic acid, 3 parts of polyvinyl alcohol and methyltrimethoxysilane together, and stir for 10 minutes to obtain a mixture 1;
[0044] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0045] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0046] S4: Pour 2 parts of polyvinyl alcohol, 2 parts of water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 300 r / min for 10 minutes until the diameter of the nano-CeO2 is 22 nm;
[0047] S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add 16 parts of water, stir at a speed of 350 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0048] Embodiment 4
[0049] A radiation-proof coating, comprising the following raw materials by weight: 50 parts of acrylic emulsion, 4 parts of ammonia water, 16 parts of acetic acid, 15 parts of water, 30 parts of methyltrimethoxysilane, 3 parts of graphene oxide, 6 parts of nano CeO2, 2 parts of ammonium chloride salt, 3 parts of polyether-modified silicone defoamer, 4 parts of polyvinyl alcohol, and 0.3 parts of sodium bicarbonate;
[0050] S1: Mix acetic acid, ammonium chloride salt and methyltrimethoxysilane together, and stir for 10 minutes to obtain a mixture 1;
[0051] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0052] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0053] S4: Pour polyvinyl alcohol, 2 parts of water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 300 r / min for 15 min until the diameter of the nano-CeO2 is 20 nm;
[0054] S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add 13 parts of water, stir at 380 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0055] Embodiment 5
[0056] A radiation-proof coating, comprising the following raw materials by weight: 70 parts of acrylic emulsion, 5 parts of ammonia water, 20 parts of acetic acid, 10 parts of water, 38 parts of methyltrimethoxysilane, 4 parts of graphene oxide, 4 parts of nano CeO2, 3 parts of polyvinyl pyrrolidone, 3 parts of ethanol, 4 parts of polyvinyl alcohol, and 0.3 parts of sodium bicarbonate;
[0057] The following steps are involved:
[0058] S1: acetic acid, polyvinyl pyrrolidone and methyltrimethoxysilane were mixed together and stirred for 10 min to obtain a mixture 1;
[0059] S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol;
[0060] S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion;
[0061] S4: Pour polyvinyl alcohol, 2 parts of water and sodium bicarbonate into nano-CeO2 and grind at a grinding speed of 250 r / min for 10 min until the diameter of the nano-CeO2 is 24 nm;
[0062] S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add 8 parts of water, stir at a speed of 400 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
[0063] The method of using the radiation protection coating of the present application is to apply it on the outside of bricks and stones with a coating thickness of 10mm-15mm, and then dry it naturally.
[0064] The following table 1 is the performance parameter table 1 of the radiation protection coating of the present embodiment 1 to 5
[0065]
[0066] The embodiments described above are only preferred implementation modes of the present invention and cannot be used to limit the protection scope of the present invention. Any non-substantial changes and modifications made by those skilled in the art on the basis of the present invention shall fall within the protection scope of the present invention.
Claims
1. A radiation protection coating, characterized in that: Includes the following ingredients in serving sizes: 50-70 parts of acrylic emulsion, 2-5 parts of ammonia water, 15-20 parts of acetic acid, 10-20 parts of water, 30-45 parts of methyltrimethoxysilane, 2-5 parts of graphene oxide, 1-7 parts of nano-CeO2, 1.5-3 parts of surfactant, 2-3 parts of defoaming agent, and 2.5-5.5 parts of dispersant.
2. The radiation protection coating according to claim 1, wherein the dispersant is polyvinyl alcohol and sodium bicarbonate.
3. A method for preparing the radiation protection coating according to claim 2, characterized in that: The following steps are involved: S1: acetic acid, a surfactant, and methyltrimethoxysilane were mixed together and stirred for 10 min to obtain a mixture 1; S2: hydrolyzing the mixture at 25°C for 4 h to obtain silica sol; S3: pouring the acrylic emulsion into the silica sol solution obtained in step S2, stirring evenly, then adding ammonia water, stirring for 5 minutes, to obtain an acrylic composite emulsion; S4: Pour polyvinyl alcohol, water and sodium bicarbonate into nano-CeO2 and grind them at a grinding speed of 200-300 r / min for 10-15 min until the diameter of the nano-CeO2 is 20nm-25nm; S5: Pour the surfactant, defoamer and ground nano-CeO2 into the acrylic composite emulsion obtained in step S3, then add water, stir at a speed of 300-400 r / min for 5 minutes, and then ultrasonicate for 5 minutes to obtain a radiation-proof coating.
Citation Information
Patent Citations
Synthesis method of cerium oxide hydrosol dispersed by PVA (Polyvinyl Alcohol)
CN102757081A
Ultrathin high-temperature-resistant thermal-insulation paint
CN104277653A
Method for modifying water-borne wood coating by hybridizing two-dimensional graphene oxide and zero-dimensional inorganic nanoparticles
CN105713519A
Preparation method of temperature-resistant ultrathin external wall insulation coating
CN106147469A
Thermal insulation and waterproof acrylic acid functional coating and preparation method thereof
CN107760139A