Multifunctional coating as well as preparation method and application thereof
By using nano phase change microcapsules and silica nanofillers modified with quaternary ammonium silane coupling agents in water-based coatings, the aging and environmental pollution problems of traditional water-based coatings under harsh conditions are solved, and antibacterial, weather-resistant and environmentally friendly are achieved multifunctional paint effects.
Patent Information
- Application Number
- CN202410915004.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional water-based coatings are prone to aging, cracking, mildew, and peeling under conditions of moisture, light, and temperature changes. They also contain high levels of volatile organic solvents that are harmful to the environment, making it difficult to meet the weather resistance and environmental protection requirements of architectural coatings.
Polyacrylate emulsion modified with nano phase change microcapsules and silica nanofiller modified with quaternary ammonium silane coupling agent are used to form a multi-functional antibacterial, corrosion-resistant and thermally conductive product through surface modification and chemical bonding. Coatings, use water as solvent to reduce VOC emissions.
It improves the antibacterial, mildew-proof, heat-resistant, and aging-resistant properties of the coating, enhances strength and scratch resistance, extends the service life, and effectively reduces environmental risks.
Smart Images

Figure BDA0004934838930000061 
Figure BDA0004934838930000081 
Figure BDA0004934838930000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a multifunctional coating and a preparation method and application thereof. Background Art
[0002] Organic coatings contain a large amount of volatile organic solvents, which not only pollute the environment, but also cause damage to organisms. Therefore, reducing the VOC content in coatings and developing water-based coatings can effectively improve the environmental protection level of coatings and meet people's needs for a better life. Water-based coatings generally use water as the medium, polymer resin as the main component, and are assisted by various additives and functional fillers to obtain multifunctional water-based coatings that meet the needs of different occasions.
[0003] However, water-based paints also have their own disadvantages. They have poor weather resistance and are prone to mold growth on the surface. In addition, most architectural coatings need to be used under relatively harsh external conditions, such as moisture, light, or drastic temperature changes. Therefore, traditional water-based paints are prone to aging, cracking, surface contamination, mold growth, etc. during use. In addition, under conditions of drastic temperature changes, the paint and the substrate are prone to peeling, causing the paint to crack and fall off.
[0004] Therefore, there is an urgent need to develop a water-based coating that is antibacterial, corrosion-resistant, and insensitive to changes in external temperature. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a multifunctional coating and a preparation method and application thereof.
[0006] In the first aspect of the present invention, the present invention proposes a multifunctional coating. According to a specific embodiment of the present invention, the coating comprises: 50 to 70 parts by weight of a polyacrylate emulsion modified by nano phase change microcapsules, 5 to 10 parts by weight of a silicon dioxide nanofiller, 1 to 2 parts by weight of a wetting agent, 1 to 2 parts by weight of a leveling agent, 1 to 2 parts by weight of a film-forming aid, 1 to 2 parts by weight of a dispersant, 1 to 2 parts by weight of a thickener, 0.5 to 1.5 parts by weight of a defoaming agent, and 20 to 30 parts by weight of deionized water.
[0007] In the second aspect of the present invention, the present invention provides a method for preparing the multifunctional coating described in the first aspect of the present invention. According to a specific embodiment of the present invention, the method comprises: mixing and stirring a nano phase change microcapsule modified polyacrylate emulsion, a silica nanofiller, a wetting agent, a leveling agent, a film-forming aid, a dispersant, a thickener, a defoaming agent and deionized water to obtain a multifunctional coating.
[0008] In the third aspect of the present invention, the present invention provides an application of the multifunctional coating described in the first aspect of the present invention. According to a specific embodiment of the present invention, the application includes use as interior and / or exterior wall coatings of buildings, and protective coatings on wood surfaces.
[0009] Beneficial effects of the present invention:
[0010] (1) By preparing surface-modified silica phase-change nano-microcapsules, the surface of the silica phase-change nano-microcapsules is made reactive, and the silica phase-change nano-microcapsules are used as raw materials for acrylic resin emulsions, and can be evenly dispersed in the emulsion, thereby overcoming the problem that traditional phase-change microcapsules are added to coatings by physical blending, and are easily precipitated in the coatings, thereby reducing the performance of the coatings;
[0011] (2) Compared with the traditional phase-change microcapsule material with an organic polymer as the shell, the phase-change microcapsule material with a silica shell used in the present invention has better thermal conductivity and strength and can withstand more drastic temperature changes;
[0012] (3) A silane coupling agent with a quaternary ammonium salt antibacterial functional group is used to modify the nano-silica filler. The modified nano-silica can not only form cross-linking points in the coating, thereby enhancing the strength, stain resistance and scratch resistance of the coating, but also the quaternary ammonium salt functional group has a broad-spectrum antibacterial ability, giving the coating a good antibacterial and mildew-proof effect;
[0013] (4) Using water as a solvent during the preparation process can effectively reduce the emission of volatile organic compounds (VOCs) and improve the environmental protection level of the coating.
[0014] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0016] Figure 1 is a SEM image of KH570 modified silica phase change nano-microcapsules prepared according to Preparation Example 1;
[0017] Figure 2 is a TEM image of nano-silica modified with a quaternary ammonium salt silane coupling agent prepared according to Preparation Example 4;
[0018] Figure 3 It is based on the surface contact angle of the coating obtained after adding different amounts of fluorinated monomers;
[0019] Figure 4It is the temperature variation curve of the coating applied to the coating obtained according to each embodiment and comparative example. DETAILED DESCRIPTION
[0020] The embodiments of the present invention are described in detail below, which are intended to be used to explain the present invention, but are not to be construed as limiting the present invention. The embodiments described below with reference to the accompanying drawings are exemplary, intended to be used to explain the present invention, but are not to be construed as limiting the present invention.
[0021] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0022] In the first aspect of the present invention, the present invention proposes a multifunctional coating. According to a specific embodiment of the present invention, the coating comprises: 50 to 70 parts by weight of a polyacrylate emulsion modified by nano phase change microcapsules, 5 to 10 parts by weight of a silicon dioxide nanofiller, 1 to 2 parts by weight of a wetting agent, 1 to 2 parts by weight of a leveling agent, 1 to 2 parts by weight of a film-forming aid, 1 to 2 parts by weight of a dispersant, 1 to 2 parts by weight of a thickener, 0.5 to 1.5 parts by weight of a defoaming agent, and 20 to 30 parts by weight of deionized water.
[0023] In some embodiments, the wetting agent is purchased from BYK Chemical, including one or more of BYK-346, BYK-349 and BYK-378.
[0024] In some embodiments, the leveling agent is purchased from BYK Chemical, including one or more of BYK-381, BYK-306 and BYK-313.
[0025] In some embodiments, the film-forming aid includes one or more of propylene glycol butyl ether, propylene glycol phenyl ether P and dodecyl alcohol ester.
[0026] In some embodiments, the dispersant is purchased from BYK Chemicals and includes one or more of BYK-151, DISPERBYK190 and DISPERBYK187.
[0027] In some embodiments, the thickener is purchased from BYK Chemical and includes one or more of RHEOBYK-M 2600VF, RHEOBYK-7601, and RHEOBYK-1000VF.
[0028] In some embodiments, the defoaming agent is purchased from BYK Chemical, including one or more of BYK-1611, BYK-1768 and BYK-1786.
[0029] In some embodiments, the solid content of the nano phase change microcapsule modified polyacrylate emulsion is 40-60 wt %.
[0030] In some embodiments, the content of the nano phase change microcapsules in the nano phase change microcapsule-modified polyacrylate emulsion is 1 to 15 wt %, preferably 5 to 10 wt %.
[0031] In some embodiments, the nano phase change microcapsules are KH570 modified silica phase change nanocapsules. By modifying the surface of the phase change material with a reactive silane coupling agent, the silica phase change nanocapsules are chemically bonded to the polyacrylate backbone, so that the silica phase change nanocapsules are more evenly and stably distributed in the coating without precipitation and separation.
[0032] In some embodiments, the particle size of the KH570 modified silica phase change nano-microcapsules is 50 to 500 nm, preferably 100 to 200 nm.
[0033] In some embodiments, the method for preparing the KH570 modified silica phase change nanocapsules comprises:
[0034] S1: dissolving the phase change material in anhydrous ethanol, performing a first stirring to obtain a first solution, adding hexadecyltrimethylammonium bromide and n-pentanol to the homogeneous solution, performing a second stirring to obtain a second solution, adding tetraethyl orthosilicate to the second solution, performing a third stirring to obtain a third solution, adding ammonia water to the third solution, performing a fourth stirring to obtain a fourth solution, and finally cooling and centrifuging the fourth solution to obtain silica phase change nano-microcapsules.
[0035] The inventors found that the silica nano-microcapsules encapsulating the phase change material can be used as the temperature regulating material of the coating. When the temperature is higher than the phase change point, the coating absorbs heat outward, and the phase change material changes from solid to liquid, delaying the temperature rise of the coating; when the temperature is lower than the phase change point, the coating releases heat outward, and the phase change material changes from liquid to solid at the phase change point, releasing heat, thereby regulating the temperature change of the coating. Compared with the traditional phase change microcapsule material with an organic polymer as the shell, the phase change microcapsule material of the present invention has better mechanical strength and thermal conductivity, making it difficult for the phase change material encapsulated inside to leak out, thereby enhancing the stability of the phase change microcapsule material during use.
[0036] In some embodiments, the reaction ratio of the phase change material, anhydrous ethanol, hexadecyltrimethylammonium bromide, n-pentanol, tetraethyl orthosilicate and ammonia water is (1-3) g: (30-80) mL: (1-4) g: (4-8) mL: (1.5-4) mL: (4-6) mL, wherein the concentration of the ammonia water is 20-25 wt%.
[0037] In some embodiments, the first stirring temperature is 50-70° C., and the time is 30-60 min.
[0038] In some embodiments, the first stirring is performed at a temperature of 50 to 80° C. for a time of 30 to 100 min.
[0039] In some embodiments, the first stirring is performed at a temperature of 50 to 80° C. for a time of 30 to 100 min.
[0040] In some embodiments, the first stirring is performed at a temperature of 50 to 80° C. for a time of 30 to 100 min.
[0041] In some embodiments, the phase change material includes paraffin, alkanes with a carbon chain length of 12 to 30 carbon atoms, fatty acids with a carbon chain length of 12 to 30 carbon atoms, polyethylene glycol with a molecular weight of 400 to 2000, and a phase change temperature of 20 to 50°C, such as 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, etc. Preferably, the phase change material is a paraffin material with a phase change temperature of about 30 to 45°C.
[0042] S2: Dispersing silica phase change nano-microcapsules in a mixed solution of ethanol and water, stirring for the fifth time, and then ultrasonicating to obtain dispersed silica phase change nano-microcapsules; mixing KH570 and deionized water, adjusting the pH and standing for hydrolysis to obtain KH570 hydrolyzate; then heating and stirring the dispersed silica phase change nano-microcapsules and the KH570 hydrolyzate in a water bath to obtain a reaction solution; finally, filtering, washing, and drying the reaction solution to obtain KH570-modified silica phase change nano-microcapsules.
[0043] In some embodiments, the addition ratio of the silica phase change nanocapsules to the mixed solution of ethanol and water is (0.5-2) g: (15-50) mL, wherein the volume ratio of ethanol to water in the mixed solution of ethanol and water is (0.5-2): (0.5-2), preferably 1:1.
[0044] In some embodiments, the fifth stirring step is performed at a temperature of 40 to 70° C. and for a time of 0.5 to 3 h.
[0045] In some embodiments, the ultrasonication time is 10 to 60 minutes.
[0046] In some embodiments, the addition ratio of the KH570 and the deionized water is (0.05-0.2) g: (5-60) mL.
[0047] In some embodiments, the end point of adjusting the pH is 4.5-6.5.
[0048] In some embodiments, the temperature of the static hydrolysis is 20-40° C., and the time is 0.5-2.0 h.
[0049] In some embodiments, the water bath heating temperature is 40-70° C., and the heating time is 0.5-4.0 h.
[0050] In some embodiments, the drying temperature is 70-90°C.
[0051] In some embodiments, the method for preparing the nano phase change microcapsule modified polyacrylate emulsion comprises:
[0052] Sa: The acrylate monomer and the nano phase change microcapsules are mixed and stirred, and then an emulsifier is added for emulsification to obtain a pre-emulsion.
[0053] In some embodiments, the acrylate monomer includes one or more of acrylic acid, butyl acrylate, hydroxyethyl acrylate, and methyl methacrylate.
[0054] In some embodiments, the acrylate monomer includes 1 to 5 parts by weight of acrylic acid, 10 to 40 parts by weight of butyl acrylate, 20 to 60 parts by weight of methyl methacrylate, and 0 to 10 parts by weight of hydroxyethyl acrylate.
[0055] As a preferred embodiment of the present invention, the acrylate monomer also includes dodecafluoroheptyl methacrylate. The inventors found that in the coating curing process, the fluorine functional group in the fluorine-containing monomer is easily enriched on the coating surface to form a coating with low surface energy; and nano-silicon dioxide (silicon dioxide phase-change nano-microcapsules, nano-silicon dioxide modified by quaternary ammonium salt silane coupling agent), not only can enhance the strength, stain resistance and scratch resistance of the coating, but also synergize with the fluorine-containing monomer to give the coating surface strong hydrophobic and oleophobic properties, effectively resist the attachment and growth of bacteria and mold on the coating surface, and also improve the antibacterial and mildew-proof effect of the coating. Further, silicon dioxide and fluorine-containing monomers also improve the heat resistance and aging resistance of the coating, and extend the service life of the coating indoors and outdoors.
[0056] In some embodiments, the acrylic acid ester monomer further includes 1 to 15 parts by weight of dodecafluoroheptyl methacrylate.
[0057] In some embodiments, the emulsifier includes one or more of OP-10 and SDS, preferably a composite emulsifier of OP-10 and SDS in a mass ratio of (1-5): (0.2-1).
[0058] Sb: The pre-emulsion, the initiator and the deionized water are mixed and reacted, and the pH is adjusted to obtain the nano phase change microcapsule modified polyacrylate emulsion.
[0059] In some embodiments, the emulsifier and the initiator react in two steps. For example, 20 to 40 wt% of the emulsifier and 20 to 40 wt% of the initiator are reacted in advance to obtain a first reaction liquid, and then 60 to 80 wt% of the emulsifier and 60 to 80 wt% of the initiator are reacted to obtain a second reaction liquid. The second reaction liquid is then added dropwise to the first reaction liquid to react, and after adjusting the pH, a nano phase change microcapsule modified polyacrylate emulsion is obtained.
[0060] In some embodiments, the initiator includes one or more of ammonium persulfate, potassium persulfate, and benzoyl peroxide.
[0061] In some embodiments, the ratio of the acrylic acid ester monomer, the nano phase change microcapsule, the emulsifier and the initiator is (40-70): (1-10): (1.5-5): (0.5-3).
[0062] The amount of deionized water added is not particularly limited, as long as the solid content in the final emulsion is between 40 and 60 wt %.
[0063] In some embodiments, the silicon dioxide nanofiller is a nano silicon dioxide modified by a quaternary ammonium salt silane coupling agent. By grafting a quaternary ammonium salt to the surface of the nano silicon dioxide, a nano silicon dioxide filler with antibacterial function is obtained, which has the broad-spectrum antibacterial and mildew-proof effects of the quaternary ammonium salt, and has the nano silicon dioxide filler to enhance the coating performance and anti-fouling performance, and solves the poor stability of small molecule quaternary ammonium salts in the coating, and the shortcomings of easy loss, thereby having better storage stability. More importantly, the use of quaternary ammonium salts as antibacterial materials can effectively avoid the high cost of adding silver in traditional coatings and the pollution problem of silver ions to the environment.
[0064] In some embodiments, the method for preparing the quaternary ammonium silane coupling agent modified nano-silica includes: dispersing the dried nano-silica in anhydrous ethanol, adding a quaternary ammonium silane coupling agent thereto for coupling reaction, cooling, centrifuging, washing, and drying to obtain quaternary ammonium silane coupling agent modified nano-silica particles.
[0065] In some embodiments, the mass ratio of the dried nano-silica to the quaternary ammonium salt silane coupling agent is (0.5-2): (0.1-2).
[0066] In some embodiments, the coupling reaction is carried out at a temperature of 60 to 80° C. and for a time of 5 to 8 hours.
[0067] In some embodiments, the average particle size of the nano-silicon dioxide is 20 to 50 nm.
[0068] In some embodiments, the quaternary ammonium salt silane coupling agent has the molecular formula
[0069]
[0070] Wherein, x is any value between 1 and 3; R1, R2, R3, R4, R5 and R6 are alkane functional groups with 1 to 4 carbon atoms.
[0071] In some embodiments, the anion of the quaternary ammonium salt silane coupling agent is one or more of chloride ion, bromide ion and iodide ion.
[0072] In the second aspect of the present invention, the present invention provides a method for preparing the multifunctional coating described in the first aspect of the present invention. According to a specific embodiment of the present invention, the method comprises: mixing and stirring a nano phase change microcapsule modified polyacrylate emulsion, a silica nanofiller, a wetting agent, a leveling agent, a film-forming aid, a dispersant, a thickener, a defoaming agent and deionized water to obtain a multifunctional coating.
[0073] In some embodiments, the mixing temperature is 30-40°C.
[0074] In some embodiments, the stirring speed is 500-1000 rpm, and the time is 0.5-1.0 h.
[0075] It should be noted that the characteristics and advantages described above for the multifunctional coating are also applicable to the method for preparing the multifunctional coating and will not be described in detail here.
[0076] In the third aspect of the present invention, the present invention provides an application of the multifunctional coating described in the first aspect of the present invention. According to a specific embodiment of the present invention, the application includes use as interior and / or exterior wall coatings of buildings, and protective coatings on wood surfaces.
[0077] It should be noted that the features and advantages described above for the multifunctional coating and the method for preparing the multifunctional coating are also applicable to this application and will not be repeated here.
[0078] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0079] The present invention is specifically described below by examples and comparative examples. The experimental methods described below, unless otherwise specified, are all routine laboratory methods. The experimental materials described below, unless otherwise specified, can all be obtained from commercial channels.
[0080] Preparation of KH570 modified silica phase change nanocapsules
[0081] Preparation Example 1
[0082] Dissolve 1g of n-octadecane in 50mL of anhydrous ethanol at 60°C for 30 minutes to form a homogeneous solution. Add 2g of CTAB and 5mL of n-pentanol, stir and disperse evenly, then add 2mL of TEOS, stir and react at 65°C for 40 minutes, then add 4mL of ammonia water (25%) and continue to react for 4 hours. Cool down and centrifuge to obtain silica phase change nano-microcapsules. Take 1g of silica phase change nano-microcapsules and disperse them in a mixed solution of 20mL of ethanol and water (ethanol: water = 1:1), stir magnetically for 1h, and then ultrasonically disperse for 15 minutes. Weigh 0.05g of KH570, add it to deionized water, adjust the pH value to 4.5-6.5 with acetic acid and sodium hydroxide, let it stand for hydrolysis for 1h, then heat and stir in a water bath for 2h, filter, wash, and dry in an oven at 80°C to obtain KH570-modified silica phase change nano-microcapsules, as shown in the SEM image. Figure 1 As shown, the phase transition temperature is 28°C, the product is white solid, and the particle size is about 120 nm.
[0083] Preparation Example 2
[0084] Dissolve 1g PEG900 in 40mL of anhydrous ethanol and stir at 50℃ for 30 minutes to form a homogeneous solution. Add 2g CTAB and 5mL n-pentanol, stir and disperse evenly, then add 3mL TEOS, stir and react at 65℃ for 1 hour, then add 5mL ammonia water (25%) and continue to react for 4 hours. Cool down and centrifuge to obtain silica phase change nano-microcapsules. Take 1g of silica phase change nano-microcapsules and disperse them in a mixed solution of 20mL ethanol and water (ethanol: water = 1: 1), stir magnetically for 1h, and then ultrasonically disperse for 15 minutes. Weigh 0.1g of KH570, add it to deionized water, adjust the pH value to 4.5-6.5 with acetic acid and sodium hydroxide, stand for hydrolysis for 1h, then heat and stir in a water bath for 2h, filter, wash, and place in an oven at 80℃ to dry to obtain KH570-modified silica phase change nano-microcapsules. The phase transition temperature is 34°C, the product is white solid, and the particle size is about 180nm.
[0085] Preparation Example 3
[0086] Dissolve 1g of stearic acid in 50mL of anhydrous ethanol and stir at 50℃ for 1 hour to form a homogeneous solution. Add 1.5g of CTAB and 4mL of n-pentanol, stir and disperse evenly, then add 2mL of TEOS, stir and react at 65℃ for 1 hour, then add 5mL of ammonia water (25%). Continue to react for 4 hours. Cool down and centrifuge to obtain silica phase change nano-microcapsules. Take 1g of silica phase change nano-microcapsules and disperse them in a mixed solution of 20mL of ethanol and water (ethanol: water = 1: 1), stir magnetically for 1h, and then ultrasonically disperse for 15 minutes. Weigh 0.05g of KH570, add it to deionized water, adjust the pH value to 4.5-6.5 with acetic acid and sodium hydroxide, stand for hydrolysis for 1h, then heat and stir in a water bath for 2h, filter, wash, and place in an oven at 80℃ to dry to obtain KH570-modified silica phase change nano-microcapsules. The phase transition temperature is 40°C, the product is white solid, and the particle size is about 90nm.
[0087] Preparation of silica nanofillers with different amino content
[0088] Preparation Example 4
[0089] Weigh 1 g of dried nano-silica (particle size 50 nm), disperse it in 20 mL of anhydrous ethanol, add 0.2 g of quaternary ammonium bromide salt-modified silane coupling agent, and after uniform dispersion, heat to reflux temperature, stir and react for 6 hours, cool, centrifuge, wash the precipitate with ethanol 3 times, and dry to obtain nano-silica particles modified with quaternary ammonium salt silane coupling agent, the TEM image of which is shown in FIG. Figure 2 shown.
[0090] Preparation Example 5
[0091] Weigh 1 g of dried nano-silica (particle size 50 nm), disperse it in 20 mL of anhydrous ethanol, add 0.5 g of quaternary ammonium bromide modified silane coupling agent thereto, disperse evenly, heat to reflux temperature, stir and react for 6 hours, cool, centrifuge, wash the precipitate with ethanol 3 times, and dry to obtain quaternary ammonium salt silane coupling agent modified nano-silica particles.
[0092] Preparation Example 6
[0093] Weigh 1 g of dried nano-silica (particle size 20 nm), disperse it in 20 mL of anhydrous ethanol, add 0.7 g of quaternary ammonium chloride modified silane coupling agent thereto, disperse evenly, heat to reflux temperature, stir and react for 8 hours, cool, centrifuge, wash 3 times with ethanol, centrifuge and dry to obtain quaternary ammonium salt silane coupling agent modified nano-silica particles.
[0094] The quaternary ammonium salt silane coupling agent modified nano-silica particles obtained in Preparation Example 4-6 were used for determination of amino content by non-aqueous titration method with hydrochloric acid ethanol standard solution, and their antibacterial effect was tested. The results are shown in Table 1, indicating that the antibacterial effect is enhanced with the increase of amino content.
[0095] Table 1
[0096]
[0097] Modified polyacrylate emulsions with different contents of nano-phase change microcapsules
[0098] Preparation Example 7
[0099] 5 parts of acrylic acid, 25 parts of butyl acrylate, 35 parts of methyl methacrylate, 5 parts of dodecafluoroheptyl methacrylate (DFMA), 6 parts of silica phase change nano-microcapsules obtained in Preparation Example 3, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified with a high-speed emulsifier to obtain a pre-emulsion.
[0100] 30 wt% of the pre-emulsion and deionized water were mixed and stirred, the temperature was raised to 70-90°C, 1 / 3 (0.1 part) of the initiator (ammonium persulfate) was added, and the mixture was reacted for 60 minutes under stirring;
[0101] To the remaining 70 wt % of the pre-emulsion, add 2 / 3 (0.2 parts) of the initiator (ammonium persulfate), stir evenly and then dropwise add to the reaction system for 45 minutes.
[0102] After the addition is completed, the reaction is carried out at 80°C for 3 hours, then the temperature is raised to 85°C, and after keeping the temperature for 30 minutes, the temperature is lowered to 30°C, ammonia water is added, and the pH is adjusted to 7-7.5 to obtain a nano phase change microcapsule modified polyacrylate emulsion with a solid content of 60%.
[0103] Preparation Example 8
[0104] 5 parts of acrylic acid, 25 parts of butyl acrylate, 35 parts of methyl methacrylate, 5 parts of dodecafluoroheptyl methacrylate (DFMA), 10 parts of silica phase change nano-microcapsules obtained in Preparation Example 3, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7 to obtain a nano phase change microcapsule modified polyacrylate emulsion.
[0105] The contents of nano phase-change microcapsules in the solid matter of the polyacrylate emulsions obtained in Preparation Examples 7 and 8 are 7.5 wt% and 12.1 wt% respectively. The higher the content of nano phase-change microcapsules, the stronger the ability to adjust the temperature of the coating.
[0106] Nano-phase change microcapsules modified polyacrylate emulsions with different glass transition temperatures
[0107] Preparation Example 9
[0108] 2 parts of acrylic acid, 15 parts of butyl acrylate, 30 parts of methyl methacrylate, 5 parts of dodecafluoroheptyl methacrylate (DFMA), 5 parts of hydroxyethyl acrylate (HEA), 10 parts of the silica nanofiller obtained in Preparation Example 4, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7 to obtain a nano phase change microcapsule modified polyacrylate emulsion with a glass transition temperature of 24.6°C.
[0109] Preparation Example 10
[0110] 1 part of acrylic acid, 10 parts of butyl acrylate, 50 parts of methyl methacrylate, 10 parts of dodecafluoroheptyl methacrylate (DFMA), 10 parts of hydroxyethyl acrylate (HEA), 10 parts of silica nanofiller obtained in Preparation Example 4, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7 to obtain a nano phase change microcapsule modified polyacrylate emulsion with a glass transition temperature of 32.4°C.
[0111] The inventors found that nano phase change microcapsule modified polyacrylate emulsions with different glass transition temperatures have an effect on the hardness of the coating, and the optimal glass transition temperature is 10.0-35.0°C.
[0112] Nano-phase change microcapsules modified polyacrylate emulsions with different surface energies
[0113] Preparation Example 11
[0114] 2 parts of acrylic acid, 20 parts of butyl acrylate, 40 parts of methyl methacrylate, 7 parts of hydroxyethyl acrylate (HEA), 10 parts of the silica nanofiller obtained in Preparation Example 4, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7 to obtain a nano phase change microcapsule modified polyacrylate emulsion.
[0115] Preparation Example 12
[0116] 2 parts of acrylic acid, 20 parts of butyl acrylate, 40 parts of methyl methacrylate, 3.5 parts of dodecafluoroheptyl methacrylate (DFMA), 5 parts of hydroxyethyl acrylate (HEA), 10 parts of the silica nanofiller obtained in Preparation Example 4, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7, that is, a nano phase change microcapsule modified polyacrylate emulsion was obtained.
[0117] Preparation Example 13
[0118] 2 parts of acrylic acid, 15 parts of butyl acrylate, 40 parts of methyl methacrylate, 9 parts of dodecafluoroheptyl methacrylate (DFMA), 5 parts of hydroxyethyl acrylate (HEA), 10 parts of the silica nanofiller obtained in Preparation Example 4, and 2 parts of emulsifier (SDS) were mixed evenly, and emulsified in a high-speed emulsifier to obtain a pre-emulsion. The rest was the same as in Preparation Example 7 to obtain a nano phase change microcapsule modified polyacrylate emulsion.
[0119] Preparation Examples 11 to 13 respectively add different amounts of fluorine-containing monomers, wherein the weight ratios of the fluorine-containing monomers in the total acrylic acid monomers are 0%, 5%, and 10%, respectively. Figure 3 As shown, from left to right are the surface contact angles of the coatings obtained in Preparation Example 11, Preparation Example 12, and Preparation Example 13, and the contact angles are 78.2°, 97.4°, and 121.5°, respectively.
[0120] Example 1
[0121] 50 parts of the nano phase change microcapsule modified polyacrylate emulsion (phase change temperature of 28°C) obtained in Preparation Example 1, 10 parts of the silica nanofiller obtained in Preparation Example 4, 2.0 parts of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.5 parts of a film-forming aid (propylene glycol butyl ether), 2 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoamer (BYK1611), and 20-30 parts of deionized water. Stir evenly to obtain a coating with a phase change temperature of 28°C.
[0122] Example 2
[0123] The nano phase change microcapsule modified polyacrylate emulsion is the nano phase change microcapsule modified polyacrylate emulsion with a phase change temperature of 34° C. in Preparation Example 2, and the rest is the same as Example 1. A coating with a phase change temperature of 34° C. is obtained.
[0124] Example 3
[0125] The nano phase change microcapsule modified polyacrylate emulsion is the nano phase change microcapsule modified polyacrylate emulsion with a phase change temperature of 40° C. in Preparation Example 3, and the rest is the same as Example 1. A coating with a phase change temperature of 40° C. is obtained.
[0126] Example 4
[0127] 60 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 13, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoaming agent (BYK1611), and 20-30 parts of deionized water were stirred evenly to obtain a coating with a surface contact angle of 121.5°.
[0128] Example 5
[0129] The silica nanofiller is the silica nanofiller obtained in Preparation Example 5, and the rest is the same as in Example 4.
[0130] Example 6
[0131] The silica nanofiller is the silica nanofiller obtained in Preparation Example 6, and the rest is the same as in Example 4.
[0132] Example 7
[0133] 80 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 8, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoamer (BYK1611), and 20-30 parts of deionized water were mixed and stirred to obtain a coating having a phase change microcapsule content of 5wt%.
[0134] Example 8
[0135] 70 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 8, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoaming agent (BYK1611), and 20-30 parts of deionized water were stirred evenly to obtain a coating with a phase change microcapsule content of 4wt%.
[0136] Example 9
[0137] 55 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 8, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoaming agent (BYK1611), and 20-30 parts of deionized water were stirred evenly to obtain a coating with a phase change microcapsule content of 3wt%.
[0138] Example 10
[0139] 60 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 7, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoaming agent (BYK1611), and 20-30 parts of deionized water were stirred evenly to obtain a coating with a phase change microcapsule content of 2wt%.
[0140] Embodiment 11
[0141] 40 parts of the nano phase change microcapsule modified polyacrylate emulsion obtained in Preparation Example 7, 5 parts of the silica nanofiller obtained in Preparation Example 4, 1.0 part of a wetting agent (BYK-346), 2 parts of a leveling agent (BYK-381), 1.0 part of a film-forming aid (propylene glycol butyl ether), 1.5 parts of a dispersant (BYK151), 1 part of a thickener (RHEOBYK-M 2600VF), 1.0 part of a defoaming agent (BYK1611), and 20-30 parts of deionized water were stirred evenly to obtain a coating with a phase change microcapsule content of 1wt%.
[0142] Comparative Example 1
[0143] The KH570 modified silica nano phase change microcapsules were replaced with silica nano phase change microcapsules without surface modification, and the rest was the same as in Example 7.
[0144] Comparative Example 2
[0145] The KH570 modified silica nano-phase change microcapsules were replaced with silica nano-phase change microcapsules without surface modification, and the rest was the same as in Example 8.
[0146] Comparative Example 3
[0147] The nano-silica modified with the quaternary ammonium salt silane coupling agent is replaced with the nano-silica not modified with the quaternary ammonium salt silane coupling agent, and the rest is the same as in Example 9.
[0148] Comparative Example 4
[0149] The nano-silica modified with the quaternary ammonium salt silane coupling agent is replaced with the nano-silica not modified with the quaternary ammonium salt silane coupling agent, and the rest is the same as in Example 10.
[0150] Comparative Example 5
[0151] The nano-silica modified with the quaternary ammonium salt silane coupling agent is replaced with the nano-silica not modified with the quaternary ammonium salt silane coupling agent, and the rest is the same as in Example 11.
[0152] The coatings of Examples 7-11 and the acrylic coatings without the addition of nano phase change microcapsules were prepared into coating samples with a certain coating thickness (200 μm). The coating samples were placed in an environment of 40°C for 8 hours and then placed at room temperature to measure the temperature of the coating. The results are as follows: Figure 4 shown.
[0153] The antibacterial properties of the coatings prepared in Examples 1-11 and Comparative Examples 1-5 are shown in Table 2. The detection method refers to the antibacterial property determination method and antibacterial effect of antibacterial coatings (paint films) (GB / T 21866-2008) to test the antibacterial properties of the coatings. Among them, Grade I means that the antibacterial property is greater than or equal to 99%, and the antibacterial durability is greater than or equal to 95%. Grade II means that the antibacterial property is greater than or equal to 95%, and the antibacterial durability is greater than or equal to 85%.
[0154] Table 2
[0155]
[0156]
[0157] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0158] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A multifunctional coating, characterized in that: The coating comprises: 50-70 parts by weight of nano phase change microcapsule modified polyacrylate emulsion, 5-10 parts by weight of silicon dioxide nanofiller, 1-2 parts by weight of wetting agent, 1-2 parts by weight of leveling agent, 1-2 parts by weight of film-forming aid, 1-2 parts by weight of dispersant, 1-2 parts by weight of thickener, 0.5-1.5 parts by weight of defoamer and 20-30 parts by weight of deionized water.
2. The multifunctional coating according to claim 1, characterized in that: The solid content of the nano phase change microcapsule modified polyacrylate emulsion is 40-60wt%; and / or, The content of nano phase change microcapsules in the nano phase change microcapsule modified polyacrylate emulsion is 1-15wt%; and / or, The nano phase-change microcapsules are KH570-modified silicon dioxide phase-change nano microcapsules.
3. The multifunctional coating according to claim 2, characterized in that: The method for preparing the KH570 modified silica phase change nano-microcapsules comprises: (1) dissolving a phase change material in anhydrous ethanol, performing a first stirring to obtain a first solution, adding hexadecyltrimethylammonium bromide and n-pentanol to the first solution, performing a second stirring to obtain a second solution, adding tetraethyl orthosilicate to the second solution, performing a third stirring to obtain a third solution, adding ammonia water to the third solution, performing a fourth stirring to obtain a fourth solution, and finally cooling and centrifuging the fourth solution to obtain silicon dioxide phase change nano-microcapsules; (2) dispersing the silica phase change nano-microcapsules in a mixed solution of ethanol and water, stirring for the fifth time, and then ultrasonicating to obtain dispersed silica phase change nano-microcapsules; mixing KH570 and deionized water, adjusting the pH and standing for hydrolysis to obtain KH570 hydrolyzate; then heating and stirring the dispersed silica phase change nano-microcapsules and the KH570 hydrolyzate in a water bath to obtain a reaction solution; finally, filtering, washing, and drying the reaction solution to obtain KH570-modified silica phase change nano-microcapsules.
4. The multifunctional coating according to claim 3, characterized in that: The phase change material includes paraffin, alkane with a carbon chain length of 12 to 30 carbon atoms, fatty acid with a carbon chain length of 12 to 30 carbon atoms, and polyethylene glycol with a molecular weight between 400 and 2000; and / or, The phase change temperature of the phase change material is 20-50°C.
5. The multifunctional coating according to claim 1, characterized in that: The method for preparing the nano phase-change microcapsule modified polyacrylate emulsion comprises: (a) mixing and stirring the acrylic acid ester monomer and the nano phase change microcapsules, and then adding an emulsifier for emulsification to obtain a pre-emulsion; (b) mixing the pre-emulsion, the initiator and the deionized water for reaction, and adjusting the pH to obtain the nano phase change microcapsule modified polyacrylate emulsion.
6. The multifunctional coating according to claim 5, characterized in that: The acrylate monomer includes one or more of acrylic acid, butyl acrylate, hydroxyethyl acrylate, and methyl methacrylate; and / or, Preferably, the acrylate monomer comprises 1 to 5 parts by weight of acrylic acid, 10 to 40 parts by weight of butyl acrylate, 20 to 60 parts by weight of methyl methacrylate and 0 to 10 parts of hydroxyethyl acrylate; and / or, The acrylic acid ester monomer further comprises 1 to 15 parts by weight of dodecafluoroheptyl methacrylate.
7. The multifunctional coating according to claim 1, characterized in that: The silica nanofiller is nanosilica modified by a quaternary ammonium salt silane coupling agent. The method for preparing the nanosilica modified by a quaternary ammonium salt silane coupling agent comprises: dispersing the dried nanosilica in anhydrous ethanol, adding a quaternary ammonium salt silane coupling agent thereto for coupling reaction, cooling, centrifuging, washing and drying to obtain nanosilica particles modified by a quaternary ammonium salt silane coupling agent.
8. The multifunctional coating according to claim 7, characterized in that: The molecular formula of the quaternary ammonium salt silane coupling agent is Wherein, x is any value from 1 to 3; R1, R2, R3, R4, R5 and R6 are alkane functional groups with carbon atoms between 1 and 4; and / or, The anion of the quaternary ammonium salt silane coupling agent is one or more of chloride ion, bromide ion and iodide ion.
9. A method for preparing the multifunctional coating according to any one of claims 1 to 8, characterized in that: The method comprises: mixing and stirring nano phase change microcapsule modified polyacrylate emulsion, silicon dioxide nanofiller, wetting agent, leveling agent, film-forming aid, dispersant, thickener, defoamer and deionized water to obtain multifunctional coating.
10. A use of the multifunctional coating according to any one of claims 1 to 8, characterized in that: The applications include interior and / or exterior coatings for buildings, protective coatings for wood surfaces.
Citation Information
Cited By
Aerogel acrylic composite board with efficient heat insulation performance and preparation method thereof