Epoxy powder coating capable of resisting long-term cathodic disbonding and preparation method of epoxy powder coating

By introducing brominated epoxy resin and isocyanate modified epoxy resin into epoxy resin, combined with phenolic curing agents and boron amine complexes, and modifying fillers, the long-term cathodic resistance of traditional epoxy powder coatings is solved. The problem of poor peeling performance significantly improves the cathodic peeling resistance and adhesion of the coating, making it suitable for anti-corrosion applications in oil and natural gas pipelines.

CN118755355AActive Publication Date: 2024-10-11LANGFANG AIGEMA XINLI MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411115816.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-11
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

Traditional epoxy powder coatings have poor resistance to cathodic stripping under long-term use and high temperature environments, making it difficult to meet the anti-corrosion needs of oil and natural gas pipelines.

Method used

It uses bisphenol A type epoxy resin, modified epoxy resin, phenolic curing agent, filler, leveling agent, degassing agent and imidazole and other components, and introduces brominated epoxy resin and isocyanate modified epoxy resin. Synergistically, phenolic curing agents and boron amine complexes are combined, as well as fillers are modified to prepare epoxy powder coatings that are resistant to long-term cathodic peeling.

Benefits of technology

Significantly improves the long-term cathodic peeling resistance of epoxy powder coatings, enhances cathodic peeling resistance and adhesion at high temperatures, improves bending performance, and meets the anti-corrosion requirements of oil and natural gas pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of powder coatings, and provides a long-term cathodic disbonding resistant epoxy powder coating and a preparation method thereof.The long-term cathodic disbonding resistant epoxy powder coating is prepared from, by weight, 40-60 parts of bisphenol A epoxy resin, 10-30 parts of modified epoxy resin, 8-15 parts of a curing agent, 15-25 parts of filler, 0.5-1.5 parts of a flatting agent, 0.1-0.5 part of a degassing agent and 0.1-0.5 part of imidazole; the modified epoxy resin comprises brominated epoxy resin and isocyanate modified epoxy resin; the curing agent comprises a phenol curing agent and a boron-amine complex. According to the technical scheme, the problem that the long-term cathodic disbonding resistance of the epoxy powder coating in the related technology is poor is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder coatings, and in particular to an epoxy powder coating resistant to long-term cathode stripping and a preparation method thereof. Background Art

[0002] For today's long-distance oil and natural gas pipelines, anti-corrosion methods include the use of paint to apply anti-corrosion coatings, cathodic protection, etc. Among them, the biggest and difficult-to-overcome bottleneck of paint coatings is that the coatings are prone to local defects, which in turn causes the corrosion of the substrate to increase. Cathodic protection without coating protection will face very high currents and lead to high costs. Therefore, the best anti-corrosion method is to combine paint coating and cathodic protection, which takes into account the cost while also having an excellent anti-corrosion solution effect, but cathodic protection requires that the coating peels off as little as possible in the presence of cathodic current.

[0003] Epoxy powder coatings are used as anti-corrosion coatings for long-distance pipelines such as oil and natural gas in the form of a single layer or 3PE structure bottom layer. Although the cathodic stripping performance of epoxy powder coatings is better than that of epoxy coal tar, coal tar enamel, etc., traditional epoxy powder coatings use dihydroamine or phenolic curing agents to cure bisphenol A epoxy resins. The short-term cathodic stripping performance is good, but as the long-distance pipelines have increasingly stringent requirements on service life and use environment, the coating needs to have the ability to maintain long-term anti-cathodic stripping performance, especially anti-cathodic stripping performance at higher temperatures. Therefore, it is necessary to develop epoxy powder coating products that are resistant to long-term cathodic stripping and high-temperature cathodic stripping. Summary of the invention

[0004] The invention provides an epoxy powder coating resistant to long-term cathodic stripping and a preparation method thereof, which solves the problem that the epoxy powder coating in the related art has poor resistance to long-term cathodic stripping.

[0005] The technical solution of the present invention is as follows: The present invention provides an epoxy powder coating resistant to long-term cathodic stripping, comprising the following components in parts by weight: 40-60 parts of bisphenol A epoxy resin, 10-30 parts of modified epoxy resin, 8-15 parts of curing agent, 15-25 parts of filler, 0.5-1.5 parts of leveling agent, 0.1-0.5 parts of degassing agent, and 0.1-0.5 parts of imidazole; The modified epoxy resin includes brominated epoxy resin and isocyanate modified epoxy resin.

[0006] As a further technical solution, the filler is one or more of titanium dioxide, silicon powder, carbon black, and fumed silica; the curing agent is a phenolic curing agent or the curing agent is a composition of a phenolic curing agent and a boron amine complex; the leveling agent is an organic silicone leveling agent and / or an acrylate leveling agent; the degassing agent is one or two of benzoin and polyethylene wax; and the boron amine complex includes one or more of a monoethylamine-boron trifluoride complex, a n-hexylamine-boron trifluoride complex, and an aniline-boron trifluoride complex.

[0007] As a further technical solution, the mass ratio of the brominated epoxy resin to the isocyanate-modified epoxy resin is 1:0.3~1.

[0008] As a further technical solution, the epoxy equivalent of the isocyanate-modified epoxy resin is 350-500 g / eq.

[0009] As a further technical solution, the epoxy equivalent of the brominated epoxy resin is greater than the epoxy equivalent of the isocyanate-modified epoxy resin.

[0010] As a further technical solution, the epoxy equivalent of the brominated epoxy resin is 620~750g / eq.

[0011] As a further technical solution, when the curing agent is a phenolic curing agent and a boron amine complex, the mass ratio of the phenolic curing agent to the boron amine complex is 1:0.1-0.3.

[0012] As a further technical solution, the boron amine complex is a n-hexylamine-boron trifluoride complex.

[0013] As a further technical solution, the filler is a sodium p-bromobenzenesulfinate modified filler.

[0014] As a further technical solution, the preparation method of the sodium p-bromobenzenesulfinate modified filler comprises the following steps: dissolving sodium p-bromobenzenesulfinate in water, mixing the mixture with the filler, and drying the mixture to obtain the sodium p-bromobenzenesulfinate modified filler; the mass ratio of the sodium p-bromobenzenesulfinate to the filler is 1:15-18.

[0015] In the present invention, the filler is modified by sodium p-bromobenzenesulfinate and then added to the epoxy resin and other components, thereby further improving the long-term cathode stripping resistance of the epoxy powder coating.

[0016] The present invention also provides a method for preparing the epoxy powder coating resistant to long-term cathode stripping, comprising the following steps: mixing the components of the epoxy powder coating, extruding, crushing and grinding to obtain the epoxy powder coating.

[0017] The working principle and beneficial effects of the present invention are: In the present invention, brominated epoxy resin and isocyanate-modified epoxy resin are introduced into epoxy resin, and the brominated epoxy resin and isocyanate-modified epoxy resin are used to cooperate with each other, thereby significantly improving the long-term cathode stripping resistance of epoxy powder coating. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In the following examples and comparative examples, The model of bisphenol A epoxy resin is 904; The model of brominated epoxy resin with epoxy equivalent weight of 210~240g / eq is YDB-228; The model of brominated epoxy resin with epoxy equivalent weight of 620~680g / eq is YDB-406; The model of brominated epoxy resin with epoxy equivalent weight of 690~750g / eq is YDB-408; The model of brominated epoxy resin with epoxy equivalent of 900~1000g / eq is YDB-410P; The isocyanate-modified epoxy resin with an epoxy equivalent weight of 350-500 g / eq was Amanda 1177HTM(V) purchased from Daqing Qinglu Langrun Technology Co., Ltd.; The model of the phenolic curing agent is Amanda 969A-2, which was purchased from Daqing Qinglu Langrun Technology Co., Ltd.

[0020] Example 1 An epoxy powder coating resistant to long-term cathodic stripping comprises the following components in parts by weight: 60 parts of bisphenol A epoxy resin, 10 parts of modified epoxy resin, 8 parts of curing agent, 6 parts of titanium dioxide, 13.3 parts of silicon powder, 0.5 parts of carbon black, 0.2 parts of fumed silica, 1 part of acrylate leveling agent, 0.5 parts of benzoin, and 0.5 parts of imidazole; The modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:0.2, the epoxy equivalent of the brominated epoxy resin is 900-1000 g / eq, and the epoxy equivalent of the isocyanate-modified epoxy resin is 350-500 g / eq; The curing agent is a phenolic curing agent; The preparation method of the epoxy powder coating resistant to long-term cathode stripping comprises the following steps: mixing the components of the epoxy powder coating, extruding, crushing and grinding to obtain the epoxy powder coating.

[0021] Example 2 An epoxy powder coating resistant to long-term cathodic stripping comprises the following components in parts by weight: 50 parts of epoxy resin, 20 parts of modified epoxy resin, 10 parts of curing agent, 6 parts of titanium dioxide, 11.4 parts of silicon powder, 0.5 parts of carbon black, 0.2 parts of fumed silica, 1 part of acrylate leveling agent, 0.5 parts of benzoin, and 0.4 parts of imidazole; The modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:0.2, the epoxy equivalent of the brominated epoxy resin is 900-1000 g / eq, and the epoxy equivalent of the isocyanate-modified epoxy resin is 350-500 g / eq; The curing agent is a phenolic curing agent; The preparation method of the epoxy powder coating resistant to long-term cathode stripping comprises the following steps: mixing the components of the epoxy powder coating, extruding, crushing and grinding to obtain the epoxy powder coating.

[0022] Example 3 An epoxy powder coating resistant to long-term cathodic stripping comprises the following components in parts by weight: 40 parts of epoxy resin, 30 parts of modified epoxy resin, 12 parts of curing agent, 6 parts of titanium dioxide, 9.6 parts of silicon powder, 0.5 parts of carbon black, 0.2 parts of fumed silica, 1 part of acrylate leveling agent, 0.5 parts of benzoin, and 0.2 parts of imidazole; The modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:0.2, the epoxy equivalent of the brominated epoxy resin is 900-1000 g / eq, and the epoxy equivalent of the isocyanate-modified epoxy resin is 350-500 g / eq; The curing agent is a phenolic curing agent; The preparation method of the epoxy powder coating resistant to long-term cathode stripping comprises the following steps: mixing the components of the epoxy powder coating, extruding, crushing and grinding to obtain the epoxy powder coating.

[0023] Example 4 The only difference between this embodiment and embodiment 3 is that the modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:0.3.

[0024] Example 5 The only difference between this embodiment and embodiment 3 is that the modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:1.

[0025] Example 6 The only difference between this embodiment and embodiment 3 is that the modified epoxy resin is a brominated epoxy resin and an isocyanate-modified epoxy resin in a mass ratio of 1:1.2.

[0026] Example 7 The only difference between this embodiment and embodiment 5 is that the epoxy equivalent of the brominated epoxy resin is 690-750 g / eq.

[0027] Example 8 The only difference between this embodiment and embodiment 5 is that the epoxy equivalent of the brominated epoxy resin is 620-680 g / eq.

[0028] Example 9 The only difference between this embodiment and embodiment 5 is that the epoxy equivalent of the brominated epoxy resin is 210-240 g / eq.

[0029] Example 10 The only difference between this embodiment and embodiment 8 is that the curing agent is a phenolic curing agent and a n-hexylamine-boron trifluoride complex in a mass ratio of 1:0.1.

[0030] Embodiment 11 The only difference between this embodiment and embodiment 8 is that the curing agent is a phenolic curing agent and a n-hexylamine-boron trifluoride complex in a mass ratio of 1:0.3.

[0031] Example 12 The only difference between this embodiment and embodiment 11 is that the filler (titanium dioxide, silicon powder, carbon black, fumed silica) is modified with sodium p-bromobenzenesulfinate, which specifically includes the following steps: dissolving 1 g of sodium p-bromobenzenesulfinate in 50 g of water, adding 16 g of the above filler, mixing, and drying to obtain a sodium p-bromobenzenesulfinate modified filler.

[0032] Comparative Example 1 The difference between this comparative example and Example 3 is that the modified epoxy resin is a brominated epoxy resin.

[0033] Comparative Example 2 The only difference between this comparative example and Example 3 is that the modified epoxy resin is an isocyanate-modified epoxy resin.

[0034] Comparative Example 3 The only difference between this comparative example and Example 3 is that no modified epoxy resin is added to the components of the epoxy powder coating.

[0035] The epoxy powder coatings prepared in Examples 1 to 12 and Comparative Examples 1 to 3 were respectively prepared according to the requirements of standard GB / T 39636-2020 "Technical Specification for Fusion-bonded Epoxy Powder External Coatings of Steel Pipelines" to obtain double-layer epoxy powder coating samples with a bottom layer thickness of 250 μm and a surface layer thickness of 350 μm. The cathode stripping resistance test was carried out at 65°C, -1.5V, and 28d. At the same time, the boiling adhesion at 75°C and 28d and the bending performance at -30°C and 3° were compared. The results are shown in the following table:

[0036] Compared with Comparative Examples 1 to 3, the epoxy powder coatings prepared in Examples 1 to 12 have better resistance to cathodic stripping, indicating that by introducing brominated epoxy resin and isocyanate-modified epoxy resin into the epoxy resin and utilizing the brominated epoxy resin and isocyanate-modified epoxy resin for synergistic effect, the long-term cathodic stripping resistance of the epoxy powder coatings is significantly improved.

[0037] Compared with Example 3, the epoxy powder coatings prepared in Examples 4 to 6 have better resistance to cathodic stripping, indicating that by changing the mass ratio of the brominated epoxy resin and the isocyanate-modified epoxy resin, the long-term cathodic stripping resistance of the epoxy powder coating is further improved; however, in Example 6, the epoxy equivalent of the brominated epoxy used is low, resulting in a decrease in the bending resistance.

[0038] Compared with Example 5, the cathodic stripping resistance of the epoxy powder coatings prepared in Examples 7 to 9 is better, but as the epoxy equivalent of the brominated epoxy decreases, the toughness of the coating film in Example 9 decreases and cracks occur. In a comprehensive comparison, the cathodic stripping resistance and bending resistance of Examples 7 to 8 are both better, especially in Example 8 when the epoxy equivalent is 620 to 680 g / eq, the cathodic stripping resistance, adhesion and bending resistance are all better.

[0039] Compared with Example 8, the epoxy powder coatings prepared in Examples 10-11 have better resistance to cathodic stripping, indicating that the compounding of phenolic curing agent and boron amine complex further improves the long-term cathodic stripping resistance of the epoxy powder coating.

[0040] Compared with Example 11, the epoxy powder coating prepared in Example 12 has better resistance to cathodic stripping, indicating that the filler is modified with sodium p-bromobenzenesulfinate and then added to the epoxy resin and other components, which further improves the long-term cathodic stripping resistance of the epoxy powder coating.

[0041] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An epoxy powder coating resistant to long-term cathodic stripping, characterized in that: The invention comprises the following components in parts by weight: 40-60 parts of bisphenol A epoxy resin, 10-30 parts of modified epoxy resin, 8-15 parts of curing agent, 15-25 parts of filler, 0.5-1.5 parts of leveling agent, 0.1-0.5 parts of degassing agent and 0.1-0.5 parts of imidazole; The modified epoxy resin includes brominated epoxy resin and isocyanate modified epoxy resin.

2. The epoxy powder coating resistant to long-term cathodic stripping according to claim 1, characterized in that: The filler is one or more of titanium dioxide, silicon powder, carbon black, and fumed silica; the curing agent is a phenolic curing agent or a composition of a phenolic curing agent and a boron amine complex; the leveling agent is an organic silicon leveling agent and / or an acrylate leveling agent; the degassing agent is one or two of benzoin and polyethylene wax; and the boron amine complex includes one or more of a monoethylamine-boron trifluoride complex, a n-hexylamine-boron trifluoride complex, and an aniline-boron trifluoride complex.

3. The epoxy powder coating resistant to long-term cathodic stripping according to claim 1, characterized in that: The mass ratio of the brominated epoxy resin to the isocyanate-modified epoxy resin is 1:0.3-1.

4. The epoxy powder coating resistant to long-term cathodic stripping according to claim 1, characterized in that: The epoxy equivalent of the isocyanate-modified epoxy resin is 350-500 g / eq.

5. The epoxy powder coating resistant to long-term cathodic debonding according to claim 4, characterized in that: The epoxy equivalent of the brominated epoxy resin is greater than the epoxy equivalent of the isocyanate-modified epoxy resin.

6. The epoxy powder coating resistant to long-term cathodic debonding according to claim 5, characterized in that: The epoxy equivalent of the brominated epoxy resin is 620-750 g / eq.

7. The epoxy powder coating resistant to long-term cathodic stripping according to claim 2, characterized in that: When the curing agent is a composition of a phenolic curing agent and a boron amine complex, the mass ratio of the phenolic curing agent to the boron amine complex is 1:0.1-0.

3.

8. The epoxy powder coating resistant to long-term cathodic debonding according to claim 1, characterized in that: The filler is a sodium p-bromobenzenesulfinate modified filler.

9. The epoxy powder coating resistant to long-term cathodic debonding according to claim 8, characterized in that: The preparation method of the sodium p-bromobenzenesulfinate modified filler comprises the following steps: dissolving sodium p-bromobenzenesulfinate in water, mixing the mixture with the filler, and drying the mixture to obtain the sodium p-bromobenzenesulfinate modified filler; the mass ratio of the sodium p-bromobenzenesulfinate to the filler is 1:15-18.

10. The method for preparing a long-term cathodic stripping resistant epoxy powder coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: The components of the epoxy powder coating are mixed, extruded, crushed, and ground to obtain the epoxy powder coating.

Citation Information

Patent Citations

  • High-performance anti-corrosion epoxy powder coating

    CN105925145A

  • Modified epoxy resin for solvent-free copper-clad plate manufacturing procedure as well as preparation and application thereof

    CN106986980A

  • Adhesive for copper-clad plates suitable for automobiles, and preparation method thereof

    CN109536099A

  • Powder coating composition having high glass transition temperature and excellent elasticity

    KR1020130033074A

  • Powder coating composition

    US20190345343A1