Long-life low-corrosion chip photoresist cleaning solution as well as preparation method and application thereof

By using a cleaning solution that combines alkaloids and alkyl sulfoxide-based organic solvents in semiconductor manufacturing, the problems of photoresist residue and high metal corrosion rates are solved, achieving efficient, low-corrosion cleaning effects and ensuring the integrity of integrated circuits. Cleanliness and stability.

CN118755533APending Publication Date: 2024-10-11ZHEJIANG AUFIRST MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410745702.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the semiconductor manufacturing process, existing cleaning solutions are difficult to effectively remove photoresist residues, and at the same time have a high corrosion rate on metal surfaces. Traditional azole corrosion inhibitors are easily adsorbed and difficult to degrade, leading to integrated circuit pollution and conductive failures.

Method used

A long-life, low-corrosion chip photoresist cleaning solution is used. Its composition includes ultrapure water, alkaloids (such as quaternary ammonium alkaloids), sulfonyl azoles and alkyl sulfoxide organic solvents. Through the alkaloids and alcohol The combination of amines and hydrogen bonding of alkyl sulfoxides with sulfonyl azoles creates a protective film that reduces metal corrosion rates and improves cleaning efficiency.

Benefits of technology

It achieves effective removal of photoresist residue at a lower temperature, reduces metal corrosion rate, avoids contamination of integrated circuits, clean and thorough cleaning effect, no need for ultrasonic treatment, long service life of the cleaning fluid and no pollutant residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755533A_ABST
    Figure CN118755533A_ABST
Patent Text Reader

Abstract

The invention relates to a long-life low-corrosion chip photoresist cleaning solution as well as a preparation method and application thereof. The long-life low-corrosion chip photoresist cleaning solution comprises the following components in parts by weight: 5-15 parts of organic strong base; 50-80 parts of an organic solvent; 0.5-2 parts of a protective agent; 10 to 30 parts of alcohol amine; and 30-50 parts of ultrapure water. According to the invention, alkaloid is adopted as organic strong base, and the cleaning effect is enhanced through combined synergistic interaction of alkaloid and alcohol amine, so that the cleaning efficiency of the photoresist is improved. By adopting the combination of the alkyl sulfoxide organic solvent and the sulfonyl azole protective agent, the metal corrosion rate is relatively low. When the cleaning fluid is used for cleaning a chip, ultrasonic treatment is not needed, various impurities on a base material can be removed only through soaking or spraying, the decontamination effect is clean and thorough, and no pollutant residues exist.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor manufacturing technology, and in particular relates to a long-life low-corrosion chip photoresist cleaning liquid and a preparation method and application thereof. Background Art

[0002] In the process of manufacturing semiconductor components, the coating, exposure and imaging of the photoresist layer are necessary process steps for the pattern manufacturing of the components. At the end of patterning, that is, after the coating, imaging, ion implantation and etching of the photoresist layer, before the next process step, the residue of the photoresist layer material needs to be completely removed. However, since the ion bombardment in the doping step will harden the polymer of the photoresist layer, the photoresist layer becomes less soluble and thus more difficult to remove.

[0003] At present, the semiconductor manufacturing industry generally uses a two-step process of dry ashing and wet etching to remove the photoresist layer, including the first step of removing most of the photoresist layer (PR) by dry ashing; the second step of removing the remaining photoresist layer by wet etching / cleaning process using a corrosion inhibitor composition, and the specific steps are generally: cleaning liquid cleaning / rinsing / deionized water rinsing. In this process, only the residual polymer photoresist layer and inorganic substances can be removed, and the metal layer cannot be attacked and damaged.

[0004] With the improvement of semiconductor manufacturing technology and the reduction of electronic device size, more and more metal copper and low-k dielectric materials are used in the semiconductor manufacturing field. Especially with the increasing popularity of copper dual damascene process, it is increasingly important to find a cleaning solution that can effectively remove etching residues while protecting low-k dielectric materials, non-metallic materials and metal materials.

[0005] Typical cleaning solutions in the prior art include: amine cleaning solutions, semi-aqueous amine (non-hydroxylamine) cleaning solutions, and fluoride cleaning solutions. Among them, the first two types of cleaning solutions are mainly used in the cleaning process of metal aluminum wires. The cleaning solutions need to be cleaned at high temperatures, generally between 60°C and 80°C, and there is a problem of high corrosion rate for metals. Although the existing fluoride cleaning solutions can be cleaned at lower temperatures (room temperature to 50°C), they still have various disadvantages. For example, the corrosion of metal and non-metal substrates cannot be controlled at the same time, causing serious corrosion of the metal surface; using traditional benzotriazole as a corrosion inhibitor for metal copper, although the etching rate of metal copper is relatively low, the traditional azole corrosion inhibitor (BTA) is not only difficult to degrade, but also not environmentally friendly to the biological system, and is easily adsorbed on the copper surface after cleaning, resulting in pollution of the integrated circuit, which will cause unforeseen conductive failures in the circuit and unsatisfactory cleaning effect.

[0006] Therefore, in order to overcome the defects of existing cleaning solutions and adapt to new cleaning requirements, such as more environmentally friendly surface adsorption of metal corrosion inhibitors, low etching rates, etc., it is urgent to find new cleaning solutions. Summary of the invention

[0007] The technical problem solved by the present invention is that the photoresist residue in the semiconductor manufacturing process has a large corrosion rate for metals, and the traditional nitrogen azole corrosion inhibitors are easily adsorbed and difficult to degrade when controlling the corrosion of the metal surface, resulting in the pollution of integrated circuits.

[0008] In view of the technical problems existing in the prior art, the present invention designs a long-life low-corrosion chip photoresist cleaning solution and its preparation method and application. It can effectively remove photoresist residues in semiconductor manufacturing processes and has a lower metal corrosion rate, effectively solving the adsorption problem of traditional nitrogen azole corrosion inhibitors in controlling metal surface corrosion.

[0009] It should be noted that, in the present invention, unless otherwise specified, the specific meaning of "including" in relation to composition limitations and descriptions includes both open-ended "including", "comprising" and similar meanings, and closed-ended "consisting of..." and similar meanings.

[0010] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions:

[0011] A long-life low-corrosion chip photoresist cleaning solution, characterized in that it comprises the following components calculated by weight:

[0012]

[0013] 30-50 parts of ultrapure water;

[0014] Wherein, the organic strong base is an alkaloid;

[0015] The protective agent is a sulfonylazole compound.

[0016] Furthermore, the alkaloids are one or more of chelerythrine, sanguinarine, chelerythrine, oxysanguinarine, and liensinium quaternium base.

[0017] Furthermore, the sulfonylazole compound is one or more of 5-methylsulfonyl-4H-1,2,4-triazole-3-amine, 3-methylsulfonyl-4-methyl-4H-1,2,4-triazole, 3-(methylsulfonyl)-1H-1,2,4-triazole, N-benzyl-3-methylsulfonyl-1H-1,2,4-triazole-5-amine, and 4-ethyl-3-(methylsulfonyl)-4H-1,2,4-triazole.

[0018] Furthermore, the alcoholamine is one or more of phytosphingosine, phytosphingosine, isopropanolamine, ethanolamine, and diethanolamine.

[0019] Furthermore, the organic solvent is an alkyl sulfoxide; the alkyl sulfoxide is one or more of n-butyl sulfoxide, di-n-dodecyl sulfoxide, dodecyl methyl sulfoxide, di-n-octyl sulfoxide, and tetramethyl sulfoxide.

[0020] The present invention also discloses a method for preparing a long-life low-corrosion chip photoresist cleaning solution, which is characterized by comprising the following steps:

[0021] Step 1: dissolving an organic strong base in ultrapure water and stirring the mixture to obtain a solution;

[0022] Step 2: At room temperature, dissolve the alcohol amine and protective agent in an organic solvent, mix well, then add the solution prepared in step 1 and continue to mix well.

[0023] The present invention also discloses a cleaning method of a long-life low-corrosion chip photoresist cleaning solution, which is characterized by comprising the following steps:

[0024] Step 1: preparing the long-life low-corrosion chip photoresist cleaning solution with ultrapure water into an aqueous solution with a mass percentage concentration of 40-55%, and then using the aqueous solution to soak a semiconductor chip at 30-50° C. for 15-30 minutes to obtain a soaked semiconductor chip;

[0025] Step 2: Rinse the soaked semiconductor chip in ultrapure water at least twice, thereby completing the cleaning process of the semiconductor chip.

[0026] The invention also discloses the use of a long-life low-corrosion chip photoresist cleaning solution in cleaning semiconductor chips.

[0027] In the present invention, in order to further optimize the effect of the cleaning solution, the components can be optimized as follows: 5-11 parts of organic strong base; 60-70 parts of organic solvent; 1-1.5 parts of protective agent; 15-25 parts of alcohol amine; 35-45 parts of ultrapure water. It can also be more preferably: 5-8 parts of organic strong base; 60-65 parts of organic solvent; 1.3-1.5 parts of protective agent; 15-20 parts of alcohol amine; 40-45 parts of ultrapure water.

[0028] In the present invention, the alkaloid is preferably lotus seed quaternary ammonium base.

[0029] The sulfonylazole compound is preferably N-benzyl-3-methylsulfonyl-1H-1,2,4-triazole-5-amine.

[0030] The alcoholamine is preferably phytosphingosine.

[0031] The alkyl sulfoxide is preferably n-butyl sulfoxide.

[0032] In the preparation method of the present invention, there is no specific requirement for the stirring speed, as long as it can be stirred evenly.

[0033] In the present invention, the combined use of alkaloids and alcohol amines plays an important role:

[0034] By using lotus seed quaternary ammonium base as an organic strong base, phytosphingosine can combine with water molecules in water to form a network structure, which can lock the lotus seed quaternary ammonium base in water to form a micellar structure, and prevent the lotus seed quaternary ammonium base from being oxidized, so that the lotus seed quaternary ammonium base can stably exert high surface activity, reduce the interfacial tension of the solution, and improve the cleaning efficiency of the photoresist.

[0035] In the present invention, the synergistic combination of sulfoxide organic solvent and sulfonylazole protective agent plays an important role:

[0036] First, alkyl sulfoxide organic solvents and sulfonylazole protective agents can combine with hydrogen bonds. The benzene ring substitution in the sulfonylazole protective agent makes the LUMO energy level more unstable, and its HOMO-LOMO gap is the smallest. The electrons of the heteroatom group are more active and combine with the empty d orbitals in the copper atom, forming a protective film on the copper surface to protect the copper from corrosion.

[0037] Secondly, the alkyl sulfoxide organic solvents can increase the diffusion rate of the sulfonylazole protective agent after hydrogen bonding, accelerate the formation of a protective film on the copper surface, and the formed protective film is denser and has a lower corrosion rate on the metal.

[0038] The present invention provides a long-life low-corrosion chip photoresist cleaning solution and a preparation method and application thereof, which have the following beneficial effects:

[0039] 1. The present invention uses alkaloids as strong organic bases, and achieves enhanced cleaning effect through the synergistic effect of the combination of alkaloids and alcohol amines. The alcohol amine can prevent the alkaloids from being oxidized, so that the alkaloids can stably exert high surface activity, reduce the interfacial tension of the solution, and improve the cleaning efficiency of the photoresist.

[0040] 2. The present invention adopts a combination of an alkyl sulfoxide organic solvent and a sulfonylazole protective agent. The alkyl sulfoxide organic solvent and the sulfonylazole protective agent can be combined by hydrogen bonding to form a protective film on the copper surface to protect the copper from corrosion. After the alkyl sulfoxide organic solvent is combined by hydrogen bonding, the diffusion rate of the sulfonylazole protective agent can be increased, and the formation of the protective film on the copper surface is accelerated. The formed protective film is more dense and has a lower corrosion rate on the metal.

[0041] 3. When the cleaning solution of the present invention is used to clean the chip, no ultrasonic treatment is required. Various impurities on the substrate can be removed only by soaking or spraying. The decontamination effect is clean and thorough, and no pollutants remain. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 : A microscope picture of a radio frequency chip after cleaning for 3 days using the cleaning solution prepared in Comparative Example 1, magnified 100 times;

[0043] Figure 2 : A microscope picture of a radio frequency chip after being cleaned for 5 days using the cleaning solution prepared in Example 1, magnified 100 times;

[0044] Figure 3 : This is a microscope picture of a copper dummy sheet after being cleaned using the cleaning solution prepared in Comparative Example 1, magnified 100 times;

[0045] Figure 4 : This is a microscope picture of the copper dummy sheet after being cleaned using the cleaning solution prepared in Example 1, magnified 100 times. DETAILED DESCRIPTION

[0046] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:

[0047] Examples 1-5 and Comparative Examples 1-5 disclose a variety of cleaning solutions, the components and mass ratios of which are shown in Table 1. The preparation method of the cleaning solution is as follows:

[0048] Step 1: dissolving an organic strong base in ultrapure water and stirring the mixture to obtain a solution;

[0049] Step 2: At room temperature, dissolve the alcohol amine and protective agent in an organic solvent, mix well, then add the solution prepared in step 1 and continue to mix well. There is no specific speed requirement.

[0050] Table 1 Example 1-Example 5

[0051]

[0052]

[0053] Table 2 Comparative Examples 1-5

[0054]

[0055] About the cleaning method of the cleaning fluid in the present invention:

[0056] Step 1: preparing a long-life low-corrosion chip photoresist cleaning solution with ultrapure water into an aqueous solution with a mass percentage concentration of 50%, then heating the aqueous solution to 40° C. and keeping it at 40° C. for 5 days for standby use; using the aqueous solution to soak a semiconductor chip at 40° C. for 25 minutes to obtain a soaked semiconductor chip;

[0057] Step 2: Rinse the soaked semiconductor chip in ultrapure water for at least two times to complete the cleaning process of the semiconductor chip.

[0058] About performance testing and description:

[0059] 1. The cleaning life test method is as follows:

[0060] The long-life low-corrosion chip photoresist cleaning solution is prepared into an aqueous solution with a mass percentage concentration of 50% by ultrapure water, and then the aqueous solution is heated to 40° C. and maintained at 40° C. for 5 days for standby use;

[0061] Soaking the radio frequency chip in the aqueous solution at 40° C. for 25 minutes to obtain a soaked radio frequency chip;

[0062] The RF chip is rinsed in ultrapure water at least twice after being soaked, thus completing the cleaning process of the RF chip.

[0063] Use a microscope to observe whether there is any residue on the surface of the semiconductor chip after cleaning. The test results are shown in Figure 1 and Figure 2 and Table 3.

[0064] 2. The test method for substrate corrosion rate is as follows:

[0065] ICP-MS (Inductively Coupled Plasma Mass Spectrometry) was used to accurately and quantitatively test the corrosion of metallic copper. The specific test method is as follows:

[0066] The size of the copper plated surface is 4×4cm 2 The Si wafer (copper dummy wafer) was immersed in a cleaning solution at 40°C for 30 min. The metal ion concentration in the cleaning solution was measured by ICP-MS, and the corrosion rate ( Right now It can also be called "etching rate"), thus investigating the corrosion rate of different cleaning solutions on metal copper. The test results are shown in Figure 3 and Figure 4 .

[0067] Table 3 Test results

[0068]

[0069]

[0070] Analysis of the test results:

[0071] Based on the contents of Table 3, it can be seen that the cleaning solutions provided in Examples 1-5 of the present invention still have good cleaning effects after 5 days, and the corrosion rate of copper is Although some cleaning solutions in the comparative example can also achieve a lower corrosion rate, they become ineffective in about 3 days and some residues remain after cleaning. Although some cleaning solutions in the comparative example do not become ineffective, their corrosion rate on copper is relatively high. In other words, the life span and corrosion rate on copper of the cleaning solutions prepared in the embodiments of the present invention are significantly improved compared with those in the comparative example.

[0072] For example, in Comparative Example 1, no lotus seed quaternary ammonium base was added, which resulted in an increase in the interfacial tension of the system, a decrease in the cleaning effect, and the presence of residues.

[0073] In Comparative Example 2, no protective agent was added. When the solution was used, it came into contact with air, causing the lotus seed quaternary ammonium base to be oxidized, resulting in a reduced service life and an increased corrosion rate of copper.

[0074] Comparative Example 3 uses sulfolane as the organic solvent, which results in an increase in the corrosion rate of the metal.

[0075] Comparative Example 4 did not add phytosphingosine, which resulted in an increased corrosion rate of the metal and the presence of more residues.

[0076] Comparative Example 5 uses tetramethylammonium hydroxide as the organic base, which results in high viscosity and surface tension of the system, unsatisfactory cleaning effect, and residue.

[0077] Further comparison is made through the attached drawings in the specification:

[0078] Figure 1 This is a microscope picture of a radio frequency chip after being cleaned for 3 days using the cleaning solution prepared in Comparative Example 1, magnified 100 times; Figure 2 This is a microscope picture of a radio frequency chip after being cleaned for 5 days using the cleaning solution prepared in Example 1, magnified 100 times.

[0079] from Figure 1 and Figure 2 It can be seen from the comparison that after cleaning for 3 days using the cleaning solution prepared in Comparative Example 1, there is residue on the surface of the RF chip, and the cleaning solution has become ineffective.

[0080] The surface of the RF chip can still be kept clean and intact after being cleaned in the tank with the cleaning solution prepared in Example 1 for 5 days. The cleaning solution prepared in the embodiment of the present invention has a longer lifespan.

[0081] Figure 3 This is a microscope picture of a copper dummy sheet after being cleaned using the cleaning solution prepared in Comparative Example 1, magnified 100 times; Figure 4 This is a microscope picture of the copper dummy sheet after being cleaned with the cleaning solution prepared in Example 1, magnified 100 times.

[0082] pass Figure 3 and Figure 4 It can be seen that the copper corrosion rate of the copper dummy sheet cleaned with the cleaning solution prepared in Comparative Example 1 is relatively high, and corrosion has occurred in multiple places on its surface.

[0083] However, the corrosion rate of copper in the copper dummy sheet cleaned with the cleaning solution prepared in Example 1 was low, and the surface layer was intact with little corrosion.

[0084] The present invention adopts alkaloids as strong organic bases, and realizes enhanced cleaning effect through the synergistic enhancement of the combination of alkaloids and alcohol amines, thereby improving the cleaning efficiency of photoresist. The present invention has a lower corrosion rate on metals by adopting a combination of alkyl sulfoxide organic solvents and sulfonylazole protective agents. When the cleaning solution of the present invention is used to clean chips, various impurities on the substrate can be removed only by soaking or spraying without ultrasonic treatment, and the decontamination effect is clean and thorough, and no pollutants remain.

[0085] The present invention is described exemplarily above in conjunction with the embodiments and drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned methods. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.

Claims

1. A long-life, low-corrosion chip photoresist cleaning solution, characterized in that: Calculated by weight, it includes the following components: Wherein, the organic strong base is an alkaloid; The protective agent is a sulfonylazole compound.

2. The long-life low-corrosion chip photoresist cleaning solution according to claim 1, characterized in that: The alkaloids are one or more of chelerythrine, sanguinarine, chelerythrine, oxysanguinarine and liensin quaternary ammonium base.

3. The long-life low-corrosion chip photoresist cleaning solution according to claim 1, characterized in that: The sulfonylazole compound is one or more of 5-methylsulfonyl-4H-1,2,4-triazole-3-amine, 3-methylsulfonyl-4-methyl-4H-1,2,4-triazole, 3-(methylsulfonyl)-1H-1,2,4-triazole, N-benzyl-3-methylsulfonyl-1H-1,2,4-triazole-5-amine, and 4-ethyl-3-(methylsulfonyl)-4H-1,2,4-triazole.

4. The long-life low-corrosion chip photoresist cleaning solution according to claim 1, characterized in that: The alcoholamine is one or more of phytosphingosine, apigenin, isopropanolamine, ethanolamine and diethanolamine.

5. The long-life low-corrosion chip photoresist cleaning solution according to claim 1, characterized in that: The organic solvent is an alkyl sulfoxide; the alkyl sulfoxide is one or more of n-butyl sulfoxide, di-n-dodecyl sulfoxide, dodecyl methyl sulfoxide, di-n-octyl sulfoxide and tetramethyl sulfoxide.

6. A method for preparing a long-life low-corrosion chip photoresist cleaning solution according to any one of claims 1 to 5, characterized in that The following steps are involved: Step 1: dissolving an organic strong base in ultrapure water and stirring the mixture to obtain a solution; Step 2: At room temperature, dissolve the alcohol amine and protective agent in an organic solvent, mix well, then add the solution prepared in step 1 and continue to mix well.

7. A method for cleaning a long-life, low-corrosion chip photoresist cleaning solution according to any one of claims 1 to 5, characterized in that The following steps are involved: Step 1: preparing the long-life low-corrosion chip photoresist cleaning solution with ultrapure water into an aqueous solution with a mass percentage concentration of 40-55%, and then using the aqueous solution to soak a semiconductor chip at 30-50° C. for 15-30 minutes to obtain a soaked semiconductor chip; Step 2: Rinse the soaked semiconductor chip in ultrapure water at least twice, thereby completing the cleaning process of the semiconductor chip.

8. Use of the long-life low-corrosion chip photoresist cleaning solution according to any one of claims 1 to 5 in cleaning semiconductor chips.