Preparation process of hot extrusion aluminum alloy profile
By using Nb2C and Ta2C raw materials and uniformly dispersed NbC and TaC powders in the hot extrusion aluminum alloy profile preparation process, combined with cold hydrogen quenching, the problem of poor mechanical properties is solved and high tensile strength and elongation are achieved. Hot extruded aluminum alloy profiles.
Patent Information
- Application Number
- CN202410731091.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-11
AI Technical Summary
The existing hot extrusion aluminum alloy profile preparation process results in insufficient mechanical properties, especially defects such as deformation and cracks during the heat treatment process.
Raw materials containing Nb2C and Ta2C are used, and NbC and TaC powders are uniformly dispersed for hot extrusion molding, and cold hydrogen is used for quenching during the quenching process to form a spatial structure with regular directions to improve mechanical properties.
Significantly improves the tensile strength and elongation of hot-extruded aluminum alloy profiles, prevents surface exudation of Nb2C and Ta2C and oxidation of C, ensuring excellent mechanical properties.
Smart Images

Figure BDA0004880235260000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy profile processing, and in particular to a preparation process of a hot extruded aluminum alloy profile. Background Art
[0002] With the development of the construction industry, people have higher requirements for the quality of raw materials, which makes professionals constantly pursue the optimization of raw material performance. Because aluminum alloy materials have high corrosion resistance and good thermal conductivity, they are widely used in modern manufacturing. As one of the common materials in the construction industry and life equipment processing fields, aluminum alloy materials have good adaptability in high temperature and high heat environments. Aluminum alloys are made into products of different shapes and structures, but the material is prone to material deformation during processing. During the processing, it is difficult to remove and take measures in a short time because the internal stress value of the aluminum alloy material cannot be further observed. After the aluminum alloy material is removed, the internal stress value changes, making it easy to deform during the production of aluminum alloy materials for complex structural products; compared with steel materials, cast aluminum alloys have the characteristics of small volume and mass, high specific strength, good corrosion resistance, good cutting performance and excellent casting performance. In order to reduce the weight of the structure and improve the performance of the production, more and more parts use cast aluminum alloy materials. Cast aluminum alloys must eventually be heat treated to obtain the required mechanical properties. Due to the large size, uneven wall thickness and complex shape of large aluminum alloy castings, their heat treatment has particularity and complexity, and it is easy to produce heat treatment defects such as unqualified mechanical properties and deformation cracks. CN115747540A discloses a preparation process for hot extruded aluminum alloy profiles, but the hot extruded aluminum alloy profiles prepared therefrom have the problem of insufficient mechanical properties.
[0003] In summary, after extensive searching by the applicant, it is found that at least there is a problem in this field that the mechanical properties of hot-extruded aluminum alloy profiles obtained by the existing preparation process of hot-extruded aluminum alloy profiles are not excellent enough. Therefore, it is necessary to develop or improve a preparation process of hot-extruded aluminum alloy profiles. Summary of the invention
[0004] Based on this, in order to solve the problem that the mechanical properties of the hot extruded aluminum alloy profiles obtained by the existing hot extruded aluminum alloy profile preparation process are not good enough, the present invention provides a hot extruded aluminum alloy profile preparation process, and the specific technical scheme is as follows:
[0005] A preparation process for a hot extruded aluminum alloy profile comprises the following steps:
[0006] Adding raw materials into a smelting furnace for smelting to obtain an aluminum alloy molten body;
[0007] Refining the aluminum alloy smelt to obtain a refined aluminum alloy;
[0008] Casting the refined aluminum alloy to obtain an aluminum alloy casting;
[0009] Hot extrusion molding the aluminum alloy casting to obtain a hot extruded casting;
[0010] quenching the hot extruded casting to obtain a quenched aluminum alloy;
[0011] Sawing the quenched aluminum alloy to obtain a sawn aluminum alloy;
[0012] Artificially aging the sawn aluminum alloy to obtain the hot extruded aluminum alloy profile;
[0013] The raw materials include Nb2C and Ta2C.
[0014] Furthermore, based on the total mass of the hot-extruded aluminum alloy profile, the raw materials include 1.1-1.5wt% Si; 1.8-2.8wt% Cu; 1.3-1.7wt% Mg; 0.1-0.5wt% Mn; 0.5-1.1wt% TiC; 1.2-2.2wt% Nb2C; 1.7-2.1wt% Ta2C; and the balance Al.
[0015] Furthermore, the smelting condition is a smelting temperature of 710-730°C.
[0016] Furthermore, the refining temperature is 710-750° C., the refining time is 10-15 min, the refining is mixed gas refining, the mixed gas is a mixed gas of argon and chlorine, and the number of refining is 2-3 times;
[0017] The volume ratio of the argon gas to the chlorine gas is 11.5-13.5:0.5-1.5.
[0018] Furthermore, the casting conditions are as follows: a casting temperature of 710 to 750° C., a casting speed of 32 to 38 mm / min, and a casting water pressure of 0.05 to 0.07 MPa.
[0019] Furthermore, the hot extrusion molding comprises the following steps:
[0020] The NbC and TaC powders are uniformly dispersed in an extrusion die, and then heated to 430-470° C. to obtain a preheated extrusion die;
[0021] Heat the extrusion barrel to 390-430°C and keep it warm for 3.3-3.7 hours to obtain a preheated extrusion barrel;
[0022] The aluminum alloy casting is preheated to 490-510° C., then added into the preheated extrusion die, and hot extrusion treatment is performed using the preheated extrusion barrel to obtain the hot extrusion casting.
[0023] Furthermore, the deformation amount of the hot extrusion treatment is 90-96%, the temperature of the hot extrusion treatment is 470-490° C., and the speed of the hot extrusion treatment is 8-10 m / min;
[0024] The mass ratio of the NbC powder, the TaC powder and the aluminum alloy casting is 0.5-1:0.5-1:103-107.
[0025] Furthermore, the quenching method is one of air cooling quenching, water spray cooling quenching and immersion cooling quenching;
[0026] The gas for air-cooling quenching is hydrogen or air.
[0027] Furthermore, the sawing conditions are preheating at 390-410° C. for 1.8-2.2 hours, and then setting the cutting head length to 0.8-0.9 m and the cutting tail length to 2.9-3.1 m.
[0028] Furthermore, the artificial aging temperature is 160-180° C., and the insulation time is 5-7 hours.
[0029] The preparation process of the hot extruded aluminum alloy profile provided by the above technical solution, because the raw materials contain TiC, Nb2C and Ta2C at the same time, the hot extruded aluminum alloy profile obtained by using uniformly dispersed NbC and TaC powders in the hot extrusion molding process, and cold hydrogen quenching during quenching, has excellent mechanical properties. Specifically, Nb2C and Ta2C have a two-dimensional layered structure, TiC (titanium carbide) has a face-centered cubic lattice, TiC, Nb2C and Ta2C and Si, Cu, Mg, Mn, and the remaining Al can form a space structure with a regular direction; further, the use of uniformly dispersed NbC and TaC powders in the hot extrusion molding process can prevent or supplement the surface seepage of Nb2C and Ta2C; further, the use of cold hydrogen quenching during quenching can prevent the oxidation of C (carbon); thus, the hot extruded aluminum alloy profile obtained by the preparation process of the hot extruded aluminum alloy profile provided by the present application has excellent tensile strength and elongation. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with its embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and do not limit the protection scope of the present invention.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0032] A preparation process of a hot extruded aluminum alloy profile in one embodiment of the present invention comprises the following steps:
[0033] Adding raw materials into a smelting furnace for smelting to obtain an aluminum alloy molten body;
[0034] Refining the aluminum alloy smelt to obtain a refined aluminum alloy;
[0035] Casting the refined aluminum alloy to obtain an aluminum alloy casting;
[0036] Hot extrusion molding the aluminum alloy casting to obtain a hot extruded casting;
[0037] quenching the hot extruded casting to obtain a quenched aluminum alloy;
[0038] Sawing the quenched aluminum alloy to obtain a sawn aluminum alloy;
[0039] Artificially aging the sawn aluminum alloy to obtain the hot extruded aluminum alloy profile;
[0040] The raw materials include Nb2C and Ta2C.
[0041] In one of the embodiments, based on the total mass of the hot-extruded aluminum alloy profile, the raw materials include 1.1-1.5wt% Si; 1.8-2.8wt% Cu; 1.3-1.7wt% Mg; 0.1-0.5wt% Mn; 0.5-1.1wt% TiC; 1.2-2.2wt% Nb2C; 1.7-2.1wt% Ta2C; and the balance Al.
[0042] In one embodiment, the smelting condition is a smelting temperature of 710-730°C.
[0043] In one embodiment, the refining temperature is 710-750° C., the refining time is 10-15 min, the refining is mixed gas refining, the mixed gas is a mixed gas of argon and chlorine, and the number of refining is 2-3 times;
[0044] The volume ratio of the argon gas to the chlorine gas is 11.5-13.5:0.5-1.5.
[0045] In one of the embodiments, the casting conditions are as follows: a casting temperature of 710-750° C., a casting speed of 32-38 mm / min, and a casting water pressure of 0.05-0.07 MPa.
[0046] In one embodiment, the hot extrusion forming comprises the following steps:
[0047] Evenly dispersing NbC and TaC powders in an extrusion die, and then heating to 430-470° C. to obtain a preheated extrusion die;
[0048] Heat the extrusion barrel to 390-430°C and keep it warm for 3.3-3.7 hours to obtain a preheated extrusion barrel;
[0049] The aluminum alloy casting is preheated to 490-510° C., then added into the preheated extrusion die, and hot extrusion treatment is performed using the preheated extrusion barrel to obtain the hot extrusion casting.
[0050] In one embodiment, the deformation amount of the hot extrusion process is 90-96%, the temperature of the hot extrusion process is 470-490°C, and the speed of the hot extrusion process is 8-10 m / min;
[0051] The mass ratio of the NbC powder, the TaC powder and the aluminum alloy casting is 0.5-1:0.5-1:103-107.
[0052] In one embodiment, the quenching method is one of air cooling quenching, water spray cooling quenching and immersion cooling quenching;
[0053] The gas for air-cooling quenching is hydrogen or air.
[0054] In one of the embodiments, the sawing conditions are preheating at 390-410° C. for 1.8-2.2 hours, and then setting the cutting head length to 0.8-0.9 m and the cutting tail length to 2.9-3.1 m.
[0055] In one embodiment, the artificial aging temperature is 160-180° C., and the holding time is 5-7 hours.
[0056] The embodiments of the present invention will be described in detail below with reference to specific examples.
[0057] Embodiment 1:
[0058] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 1.9wt% Ta2C, and the remainder Al are mixed uniformly to obtain the raw materials;
[0059] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0060] Embodiment 2:
[0061] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 1.7wt% Ta2C, and the remainder Al are mixed uniformly to obtain the raw materials;
[0062] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0063] Embodiment 3:
[0064] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 2.1wt% Ta2C, and the remainder Al are uniformly mixed to obtain the raw materials;
[0065] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0066] Comparative Example 1:
[0067] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% NbC, 2.1wt% TaC, and the remainder Al are mixed uniformly to obtain the raw materials;
[0068] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0069] Comparative Example 2:
[0070] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 2.1wt% TaC, and the remainder Al are mixed uniformly to obtain the raw materials;
[0071] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0072] Comparative Example 3:
[0073] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.9wt% Ta2C, 1.7wt% NbC, and the remainder Al are uniformly mixed to obtain a raw material;
[0074] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0075] Comparative Example 4:
[0076] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 1.9wt% Ta2C, and the remainder Al are mixed uniformly to obtain the raw materials;
[0077] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; heating the extrusion die to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; The aluminum casting is preheated to 500° C., and then added to the preheated extrusion die, and the preheated extrusion barrel is used for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480° C., and the speed of the hot extrusion treatment is 9m / min; the hot extruded casting is cold hydrogen quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400° C. for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170° C., and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0078] Comparative Example 5:
[0079] Preparation of raw materials: Based on the total mass of the hot extruded aluminum alloy profile, 1.3wt% Si, 2.3wt% Cu, 1.5wt% Mg, 0.3wt% Mn, 0.8wt% TiC, 1.7wt% Nb2C, 1.9wt% Ta2C, and the remainder Al are mixed uniformly to obtain the raw materials;
[0080] Preparation of hot extruded aluminum alloy profiles: adding the above raw materials into a smelting furnace and smelting at 720°C to obtain an aluminum alloy smelt; refining the aluminum alloy smelt, setting the refining temperature to 730°C, introducing a mixed gas of argon and chlorine for refining for 12 minutes, wherein the volume ratio of argon to chlorine is 12.5:1, repeating the refining twice to obtain a refined aluminum alloy; casting the refined aluminum alloy at a temperature of 730°C and a water pressure of 0.06MPa at a speed of 35mm / min to obtain an aluminum alloy casting; uniformly dispersing NbC and TaC powders in an extrusion die, and then heating to 450°C to obtain a preheated extrusion die; heating the extrusion barrel to 410°C and keeping it warm for 3.5h to obtain a preheated extrusion barrel; preheating the above aluminum alloy casting to 500 ℃, and then add it into the above-mentioned preheated extrusion die, use the above-mentioned preheated extrusion barrel for hot extrusion treatment to obtain a hot extruded casting, wherein the conditions for the hot extrusion treatment are that the deformation amount of the hot extrusion treatment is 95%, the temperature of the hot extrusion treatment is 480℃, the speed of the hot extrusion treatment is 9m / min, and the mass ratio of NbC powder, TaC powder and aluminum alloy casting is 0.7:0.8:105; the hot extruded casting is cold air quenched to obtain a quenched aluminum alloy; the quenched aluminum alloy is sawed, and the sawing conditions are preheating at 400℃ for 2h, and then setting the cutting head length to 0.9m and the cutting tail length to 3.1m to obtain a sawed aluminum alloy; the sawed aluminum alloy is artificially aged, the artificial aging temperature is 170℃, and the insulation time is 6h to obtain a hot extruded aluminum alloy profile.
[0081] The hot extruded aluminum alloy profiles obtained in Examples 1 to 3 and Comparative Examples 1 to 5 were tested for tensile strength and elongation. The test results are shown in Table 1.
[0082] Table 1:
[0083]
[0084]
[0085] As can be seen from Table 1, the preparation process of the hot extruded aluminum alloy profile provided by Examples 1 to 3, because the raw materials contain TiC, Nb2C and Ta2C at the same time, uniformly dispersed NbC and TaC powders are used in the hot extrusion molding process, and cold hydrogen quenching is used during quenching, the mechanical properties of the hot extruded aluminum alloy profile obtained, namely, excellent tensile strength and elongation. Specifically, Nb2C and Ta2C have a two-dimensional layered structure, TiC (titanium carbide) has a face-centered cubic lattice, TiC, Nb2C and Ta2C and Si, Cu, Mg, Mn, and the remaining Al can form a space structure with a regular direction; further, the use of uniformly dispersed NbC and TaC powders during hot extrusion molding can prevent or supplement the surface seepage of Nb2C and Ta2C; further, the use of cold hydrogen quenching during quenching can prevent the oxidation of C (carbon); thus, the hot extruded aluminum alloy profile obtained by the preparation process of the hot extruded aluminum alloy profile provided by the present application has excellent tensile strength and elongation.
[0086] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A process for preparing a hot extruded aluminum alloy profile, characterized in that: It includes the following steps: Adding raw materials into a smelting furnace for smelting to obtain an aluminum alloy molten body; Refining the aluminum alloy smelt to obtain a refined aluminum alloy; Casting the refined aluminum alloy to obtain an aluminum alloy casting; Hot extrusion molding the aluminum alloy casting to obtain a hot extruded casting; quenching the hot extruded casting to obtain a quenched aluminum alloy; Sawing the quenched aluminum alloy to obtain a sawn aluminum alloy; Artificially aging the sawn aluminum alloy to obtain the hot extruded aluminum alloy profile; The raw materials include Nb2C and Ta2C.
2. The preparation process according to claim 1, characterized in that: Taking the total mass of the hot extruded aluminum alloy profile as 100%, the raw materials include 1.1-1.5wt% Si; 1.8-2.8wt% Cu; 1.3-1.7wt% Mg; 0.1-0.5wt% Mn; 0.5-1.1wt% TiC; 1.2-2.2wt% Nb2C; 1.7-2.1wt% Ta2C; and the balance Al.
3. The preparation process according to claim 1, characterized in that: The smelting condition is a smelting temperature of 710-730°C.
4. The preparation process according to claim 1, characterized in that: The refining temperature is 710-750°C, the refining time is 10-15 minutes, the refining is mixed gas refining, the mixed gas is a mixed gas of argon and chlorine, and the number of refining is 2-3 times; The volume ratio of the argon gas to the chlorine gas is 11.5-13.5:0.5-1.
5.
5. The preparation process according to claim 1, characterized in that: The casting conditions are as follows: a casting temperature of 710 to 750° C., a casting speed of 32 to 38 mm / min, and a casting water pressure of 0.05 to 0.07 MPa.
6. The preparation process according to claim 1, characterized in that: The hot extrusion molding comprises the following steps: Evenly dispersing NbC and TaC powders in an extrusion die, and then heating to 430-470° C. to obtain a preheated extrusion die; Heat the extrusion barrel to 390-430°C and keep it warm for 3.3-3.7 hours to obtain a preheated extrusion barrel; The aluminum alloy casting is preheated to 490-510° C., then added into the preheated extrusion die, and hot extrusion treatment is performed using the preheated extrusion barrel to obtain the hot extrusion casting.
7. The preparation process according to claim 6, characterized in that: The deformation amount of the hot extrusion treatment is 90-96%, the temperature of the hot extrusion treatment is 470-490°C, and the speed of the hot extrusion treatment is 8-10m / min; The mass ratio of the NbC powder, the TaC powder and the aluminum alloy casting is 0.5-1:0.5-1:103-107.
8. The preparation process according to claim 1, characterized in that: The quenching method is one of air cooling quenching, water spray cooling quenching and immersion cooling quenching; The gas for air-cooling quenching is hydrogen or air.
9. The preparation process according to claim 1, characterized in that: The sawing conditions are preheating at 390-410° C. for 1.8-2.2 hours, and then setting the cutting head length to 0.8-0.9 m and the cutting tail length to 2.9-3.1 m.