Boron-containing die-casting aluminum alloy and preparation method and application thereof
By optimizing the composition of Si, Fe, Mn, Mg, B and Al-Sr-RE, combined with aging treatment, the problem of insufficient strength and plasticity of existing die-cast aluminum alloys was solved, and a boron-containing die-cast aluminum alloy with high strength and toughness was prepared, which is suitable for in the field of automotive lightweighting.
Patent Information
- Application Number
- CN202410783714.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing die-cast aluminum alloy materials have limitations in improving strength and plasticity, especially the insufficient rigidity of large-size castings. Too high Fe and Mn content can easily form coarse primary iron-rich phases, which is not conducive to plasticity improvement. High Cu content has a tendency of hot cracking. , and the absence of grain refiner limits the improvement of alloy strength and toughness.
Boron-containing die-cast aluminum alloy is used. By optimizing the composition of Si, Fe, Mn, Mg, B and Al-Sr-RE, designing high Si content to ensure die-casting performance, controlling the total amount of Fe and Mn, and adding Mg for solid solution strengthening. B is used to refine the grains, and Al-Sr-RE is used to deeply modify the eutectic silicon, inhibit the formation of Mg2Si, and improve the tensile strength and yield strength through aging treatment.
A boron-containing die-cast aluminum alloy with high strength and toughness has been achieved, with a tensile strength of 290 to 340MPa, a yield strength of 130 to 200MPa, and an elongation of 13 to 20%. It is suitable for the field of automobile lightweighting.
Smart Images

Figure CN118756008A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and in particular relates to a boron-containing die-casting aluminum alloy and a preparation method and application thereof. Background Art
[0002] In recent years, die-casting integrated molding technology has become one of the effective ways to achieve lightweight automobiles, but large-sized castings often cannot be improved in strength through conventional T6 (high-temperature solid solution + artificial aging), resulting in insufficient rigidity of the castings, limiting the lightweight effect of integrated die-casting. At present, die-casting aluminum alloy materials have become an important part of integrated die-casting molding technology, and the development of high-strength and toughness die-casting aluminum alloy materials with high strength and plasticity without / non-heat treatment is the focus of research today.
[0003] Al-Si is a commonly used heat-treatment-free die-casting aluminum alloy material, including Alcoa's C611 and C891, and Rheinfeld's Castasil37 alloy. In order to ensure good elongation of the casting, the content of strengthening elements in the alloy is low, resulting in the alloy yield strength usually not higher than 125MPa. Based on this, existing research improves the strength and toughness of the alloy by refining, modifying and increasing the dispersed phase. For example: CN117845107A discloses a heat-treatment-free die-casting aluminum alloy, including: Si6.3~9.0%, Mg0.15~0.5%, Cu0.15~0.6%, Fe0.10~0.25%, Mn0.5~0.75%, Ti0.05~0.25%, Sr0.02~0.06%, Zr≤0.15%, Sb≤0.30%, less than or equal to 0.05% of other impurity elements and the balance of Al. By using Sr-Sb-Zr composite refined metamorphic structure, the tensile strength, yield strength and elongation of the casting body sample are obtained to reach 285MPa, 141MPa and 11.1% or more respectively. CN117684053A discloses a near-eutectic die-casting aluminum-silicon alloy material without heat treatment and its preparation method, including Si: 9.6-11.8%; Fe: ≤0.15%; Cu: ≤0.03%; Mn: 0.3-0.8%; Mg: 0-0.2%; Zn: ≤0.05%; Ti: 0-0.15%; Zr: 0-0.25%; rare earth 0-0.2%; Sr: 0 .01-0.05%; Pb: ≤0.1%; Sn: ≤0.01%; Cd: ≤0.01%; seed or modifier 0.05%-0.5%, the rest is Al, the seed is TCB seed, the modifier is Al-Sr-RE composite alloy, the prepared heat treatment-free alloy has a die-cast tensile strength and a yield strength of 283MPa and 125MPa or more respectively, and an elongation of not less than 13%. CN117512414A discloses a heat-free die-cast aluminum alloy based on recycled aluminum, including: Si8.0-10.5%, Fe≤0.2%, Cu≤0.20%, Mn0.4-0.8%, Mg<0.20%, Ti≤0.15%, Zn<0.15%, Ca≤20ppm, P≤20ppm, Sr0.01-0.04%, Zr0.1-0.30%; the rest are Al and unavoidable impurity elements, and the total content of unavoidable impurity elements is ≤0.15%. The obtained die-cast alloy has a strength of more than 300MPa, a yield strength of more than 160MPa, and an elongation of more than 15%. The above three heat-free treatments have good comprehensive mechanical properties, but the Fe content requirement is low, and it is impossible to test recycled aluminum with lower grade, and the comprehensive cost is high.
[0004] For example, CN116770135A discloses a high-vacuum die-cast aluminum alloy that does not require heat treatment. The high-vacuum die-cast aluminum alloy that does not require heat treatment includes, in terms of mass percentage, Si6-8%, Fe0.5-0.6%, Mn0.6-0.8%, Mg0.3-0.4%, Cu0.6-0.9%, Ti0.1-0.2%, Sr0.02-0.05%, and the remainder is Al and unavoidable impurities. The tensile strength, yield strength and elongation of the prepared die-cast alloy reach 275MPa, 145MPa and 10.5%, respectively. CN114855036A discloses a high-strength and high-thermal-conductivity cast aluminum alloy, a preparation method thereof, and an aluminum alloy product, comprising 8.5-9.5% Si, 0.4-0.65% Fe, 0.2-0.45% Mn, 0.1-0.2% Mg, 0.01-0.05% Sr, 0.02-0.08% RE, and impurity elements <0.15%, with the remainder being Al; Al-Sr-RE composite modifier is used to deeply modify eutectic silicon to improve the comprehensive mechanical properties of the alloy. The tensile strength, yield strength, and elongation of the prepared die castings reach 290MPa, 170MPa, and 10.5%, respectively. These two heat-treatment-free materials contain a relatively high content of Fe, which can meet the requirements for recycled aluminum. However, the Fe and Mn contents in CN116770135A are too high, which easily forms a coarse primary iron-rich phase, which is not conducive to improving plasticity, and contains a high content of Cu, which has a certain tendency to hot cracking. CN114855036A does not add a grain refiner, which limits the improvement of the strength and toughness of the alloy. Summary of the invention
[0005] In order to overcome at least one of the problems existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a boron-containing die-casting aluminum alloy having good strength and toughness.
[0006] A second object of the present invention is to provide a method for preparing the above-mentioned boron-containing die-casting aluminum alloy.
[0007] A third object of the present invention is to provide an application of the above-mentioned boron-containing die-casting aluminum alloy in the automotive field.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] The first aspect of the present invention provides a boron-containing die-casting aluminum alloy, which is composed of the following components in mass percentage: 8-11% Si, 0.45-0.65% Fe, 0.15-0.45% Mn, 0.1-0.25% Mg, 0.015-0.025% B, 0.01-0.025% Sr, 0.02-0.05% RE, and the remainder is impurity elements and Al; the sum of the mass percentages of Mn and Fe is 0.7-1.0%; and the Sr and RE are added in the form of an Al-Sr-RE master alloy.
[0010] The present invention is based on a hypoeutectic Al-Si alloy. In order to ensure that the alloy has good die-casting performance, a higher Si content is designed. The higher the Si content, the better the casting performance. However, as a brittle phase, the presence of Si has a certain harm to the plasticity of the alloy, so it is necessary to control the Si content within a certain range. In order to ensure good demoulding performance, it is necessary to control the total amount of Fe and Mn, and through thermodynamic calculations, the volume fraction of the solid-liquid phase in the eutectic point composition under different Si contents and the initial formation temperature of the iron-rich phase in the alloy with different Fe and Mn contents are analyzed to make it close to the eutectic temperature, and finally determine the optimized Mn and Fe element range; adding Mg is beneficial to improving the strength of the alloy through solid solution strengthening, but in order to inhibit Mg 2 The formation of Si requires the Mg content to be kept at a low level; adding B is beneficial to grain refinement, and adding Al-Sr-RE is beneficial to deep modification of eutectic silicon, thereby improving the strength and plasticity of the alloy through grain refinement and second phase refinement. Since V and Ti that may be contained in impurity elements will cause the loss of B element, the amount of B added needs to be appropriately increased.
[0011] In the composition of the boron-containing die-casting aluminum alloy, non-limiting examples of the mass percentage of Si are 8.5%, 9%, 9.5%, 10% or 10.5%.
[0012] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of Fe are 0.5%, 0.55% or 0.6%.
[0013] Preferably, in the composition of the die-cast aluminum alloy, the mass percentage of Fe is 5.2-6.8% of the mass percentage of Si; non-limiting examples are 5.5%, 5.8%, 6%, 6.2% or 6.5%. The Fe addition amount and the Si addition amount need to be kept within a certain ratio range. If the addition amounts of the two do not match, a coarse needle-shaped β-Fe phase will be formed, resulting in a significant reduction in the plasticity and strength of the alloy.
[0014] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of Mn are 0.2%, 0.25%, 0.3%, 0.35% or 0.4%.
[0015] Preferably, in the composition of the die-casting aluminum alloy, the sum of the mass percentages of Mn and Fe is 0.8-0.9%, with non-limiting examples being 0.82%, 0.85% or 0.88%.
[0016] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of Mg are 0.12%, 0.15%, 0.18%, 0.2% or 0.22%.
[0017] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of B are 0.018%, 0.02% or 0.022%.
[0018] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of Sr are 0.011%, 0.012%, 0.015%, 0.018%, 0.02% or 0.022%.
[0019] Preferably, in the composition of the die-cast aluminum alloy, the sum of the mass percentages of B and Sr does not exceed 0.04%; further preferably, the sum of the mass percentages of B and Sr is 0.02-0.039%; non-limiting examples are 0.025%, 0.026%, 0.027%, 0.03%, 0.035% or 0.037%. If the content of B and Sr is too high, the two elements will react to form a compound.
[0020] In the composition of the die casting aluminum alloy, non-limiting examples of the mass percentage of RE are 0.025%, 0.03%, 0.035%, 0.04% or 0.045%.
[0021] Preferably, in the Al-Sr-RE master alloy, the sum of the mass percentages of Sr and RE does not exceed 16%, with non-limiting examples being 10%, 12%, 13.5% or 15%.
[0022] The total addition amount of Sr and RE needs to be controlled within a certain ratio. If the amount is too high, the dissolution temperature of Al-Sr-RE will be too high, which is not conducive to the preparation of the alloy.
[0023] Preferably, the RE is a mixture of La and Ce.
[0024] Preferably, in the RE, the mass ratio of Ce to La is 2-6.
[0025] Preferably, in the composition of the die-cast aluminum alloy, the mass percentage of impurity elements is less than 0.25%; further preferably, in the impurity elements, the mass percentage of a single impurity element is less than 0.1%.
[0026] Preferably, the impurity elements include one or two elements of V and Ti, or do not include V and Ti.
[0027] Preferably, the composition of the die-casting aluminum alloy has the following relationship: B =0.01%+0.25(W V +W Ti ), W B , W V , W Ti Represent the mass percentages of B, V and Ti respectively. V Zero or non-zero, when the impurity elements include V, W V Not zero, when the impurity elements do not include V, W V Zero; W Ti Zero or non-zero, when the impurity elements include Ti, W Ti Not zero, when the impurity elements do not include Ti, W Ti is zero.
[0028] Since V and Ti elements will cause loss of B element, it is necessary to consider the content of V and Ti in the alloy raw materials and appropriately increase the amount of B added.
[0029] Preferably, the properties of the boron-containing die-cast aluminum alloy meet the following conditions: tensile strength is 290-340 MPa; yield strength is 130-200 MPa; elongation is 13-20%.
[0030] Preferably, the properties of the boron-containing die-cast aluminum alloy meet the following conditions: tensile strength of 300-340 MPa; yield strength of 160-200 MPa; elongation of 13-18%. Aging treatment is beneficial to obtain aluminum alloy materials with high tensile strength and yield strength, but plasticity will be reduced.
[0031] Preferably, the die-casting aluminum alloy contains spherical eutectic silicon grains.
[0032] Preferably, the average particle size of the eutectic silicon grains is 0.1 to 5 μm; more preferably, it is 0.1 to 3 μm; and even more preferably, it is 0.1 to 2 μm.
[0033] The second aspect of the present invention provides a method for preparing the boron-containing die-casting aluminum alloy described in the first aspect of the present invention, comprising the following steps: melting a raw material containing Si, Fe, and Mn, adjusting the content of Si, Fe, and Mn to a target content, refining, adjusting the content of B to a target content, keeping warm, adjusting the content of Mg, Sr, and RE to a target content, degassing, and casting to obtain the boron-containing die-casting aluminum alloy.
[0034] Preferably, the melting temperature is 750-800°C.
[0035] Preferably, the refining temperature is 720-760°C.
[0036] Preferably, the refining time is 10 to 20 minutes.
[0037] Preferably, the refining is carried out under the conditions of a refining agent and a protective gas.
[0038] Preferably, in the refining, the refining agent is a chloride salt refining agent.
[0039] Preferably, during the refining, the protective gas includes at least one of nitrogen, argon or helium.
[0040] Preferably, the degassing is performed in the presence of a covering agent; the covering agent is preferably a chloride.
[0041] Preferably, a step of standing still is included before the casting; the standing still time is preferably 15 to 30 minutes.
[0042] In some specific embodiments of the present invention, the content of a component is adjusted by adding a regulating raw material; the regulating raw material includes at least one of a simple substance, an intermediate alloy or a compound containing the component.
[0043] Preferably, the method for adjusting the B content is to add Al-B master alloy.
[0044] Preferably, the Mg content is regulated by adding Mg alone or Al-Mg master alloy.
[0045] Preferably, the method for adjusting the contents of Sr and RE is to add Al-Sr-RE master alloy.
[0046] Preferably, in the method for preparing the boron-containing die-casting aluminum alloy, an aging treatment step is also included after the casting.
[0047] Aging treatment is beneficial to obtain aluminum alloy materials with higher tensile strength and yield strength, but the plasticity will be reduced.
[0048] Preferably, the temperature of the aging treatment is 180-220°C; more preferably, 190-210°C.
[0049] Preferably, the aging treatment time is 30 to 50 minutes; more preferably, it is 35 to 45 minutes.
[0050] The third aspect of the present invention provides an application of the boron-containing die-casting aluminum alloy described in the first aspect of the present invention in the automotive field.
[0051] Preferably, the automobile is a lightweight automobile; further preferably, the lightweight automobile is a new energy automobile.
[0052] The beneficial effects of the present invention are as follows: the present invention is based on a hypoeutectic Al-Si alloy, and carries out alloy composition optimization design and microstructure refinement research, and gives the alloy good die-casting performance and plasticity by a specific content of Si, and regulates the Fe and Mn contents based on the Si content, so that the alloy has good demoulding properties and toughness, and solid solution strengthening, grain refinement and second phase refinement are carried out by the action of specific contents of Mg, B and Al-Sr-RE, so that the strength and plasticity of the alloy are effectively improved, and finally a high-strength and toughness boron-containing die-casting aluminum alloy is prepared, which has a wide range of applications in automobiles, especially in the field of lightweighting.
[0053] More specifically, compared with the prior art, the present invention has the following advantages:
[0054] 1. The strength and plasticity of the alloy are mainly achieved by adding strengthening elements and refining the structure. On the one hand, by designing a trace amount of Mg, the alloy strength is improved through solid solution strengthening. On the other hand, B is used to refine the grains, and Al-Sr-RE is used to deeply modify eutectic silicon to improve the alloy strength through grain refinement and second phase refinement. In order to inhibit Mg 2 In order to form Si, the Mg content is designed to be at a low level; in order to reduce the loss of B element by V and Ti, the content of V and Ti in the alloy raw materials is considered, and the addition amount of B is appropriately increased; Al-Sr-RE has been proven to have a deep metamorphic effect on eutectic silicon. Fine eutectic silicon can be obtained by adding a trace amount of Al-Sr-RE, which has a significant effect on improving the strength and plasticity of the alloy.
[0055] 2. The boron-containing die-casting aluminum alloy prepared by the present invention has a tensile strength, a yield strength and an elongation of 290-320 MPa, 130-160 MPa and 15-20% respectively without heat treatment; and after aging treatment, the tensile strength, yield strength and elongation of the casting reach 300-340 MPa, 160-200 MPa and 13-18% respectively. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 This is the metallographic spectrum of the boron-containing die-cast aluminum alloy in the die-cast state according to Example 1 of the present invention.
[0057] Figure 2 This is the tensile curve of the boron-containing die-cast aluminum alloy in the die-cast state according to Example 1 of the present invention. DETAILED DESCRIPTION
[0058] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.
[0059] It should be noted that in the following examples and comparative examples, RE is a mixture of La and Ce, and the mass ratio of Ce to La is 2 to 6; the refining agent is a chloride salt refining agent; and the covering agent is a chloride used to protect the melt.
[0060] Example 1
[0061] A boron-containing die-casting aluminum alloy, comprising the following components in percentage by mass:
[0062] Si 10%, Fe 0.65%, Mn 0.25%, Mg 0.10%, B 0.025%, Sr 0.012%, RE 0.02%, the balance is inevitable impurity elements and aluminum. RE is a mixture of La and Ce, and the mass ratio of Ce to La is 6.
[0063] The preparation process of the boron-containing die-casting aluminum alloy is as follows:
[0064] (1) Melting: Add raw materials containing Si, Fe, and Mn into a melting furnace and melt them at 760°C. After the raw materials are melted, take samples to test the alloy composition, and adjust the content of Si, Fe, and Mn alloy elements. The content of elements such as Ti and V is about 0.02%.
[0065] (2) Refining and grain refinement: The melt temperature was adjusted to 720°C, and then a high-purity inert gas containing a mixed chloride salt refining agent was introduced into the melt for 15 min; then an Al-B master alloy with a B content of 0.013% was added.
[0066] (3) Composite modification: After standing and keeping warm for 50 minutes, remove the surface slag; then add industrial pure Mg and Al-Sr-RE composite modifier, sprinkle a layer of covering agent on the surface of the melt, and pass preheated inert gas for degassing for 10 minutes.
[0067] (4) Casting: After the melt is left to stand for 30 minutes, the dewatering port is opened and the melt is directly supplied to the die-casting equipment or ingot through the flow trough. An online rotary degassing box and a ceramic filter plate can be installed in the flow trough to obtain high-quality castings or ingots.
[0068] Example 2
[0069] A boron-containing die-casting aluminum alloy, comprising the following components in percentage by mass:
[0070] Si 9.0%, Fe 0.50%, Mn 0.35%, Mg 0.25%, B 0.015%, Sr 0.011%, RE 0.05%, the balance is inevitable impurity elements and aluminum. RE is a mixture of La and Ce, and the mass ratio of Ce to La is 4.
[0071] The preparation process of the boron-containing die-casting aluminum alloy is as follows:
[0072] (1) Melting: Add raw materials containing Si, Fe, and Mn into a melting furnace and melt them at 780°C. After the raw materials are melted, take samples to test the alloy composition, and adjust the content of Si, Fe, and Mn alloy elements. The content of elements such as Ti and V is about 0.03%.
[0073] (2) Refining and grain refinement: The melt temperature was adjusted to 740°C, and then a high-purity inert gas containing a mixed chloride salt refining agent was introduced into the melt for 15 min; then an Al-B master alloy with a B content of 0.018% was added.
[0074] (3) Composite modification: After standing and keeping warm for 40 minutes, remove the surface slag; then add industrial pure Mg and Al-Sr-RE composite modifier, sprinkle a layer of covering agent on the surface of the melt, and pass preheated inert gas for degassing for 10 minutes.
[0075] (4) Casting: After the melt is left to stand for 20 minutes, the dewatering port is opened and the melt is directly supplied to the die-casting equipment or ingot through the flow trough. An online rotary degassing box and a ceramic filter plate can be installed in the flow trough to obtain high-quality castings or ingots.
[0076] Example 3
[0077] A boron-containing die-casting aluminum alloy, comprising the following components in percentage by mass:
[0078] Si 8.0%, Fe 0.45%, Mn 0.40%, Mg 0.20%, B 0.02%, Sr 0.015%, RE 0.03%, the balance is inevitable impurity elements and aluminum. RE is a mixture of La and Ce, and the mass ratio of Ce to La is 3.
[0079] The preparation process of the boron-containing die-casting aluminum alloy is as follows:
[0080] (1) Melting: Add raw materials containing Si, Fe, and Mn into a melting furnace and melt them at 800°C. After the raw materials are melted, take samples to test the alloy composition, and adjust the content of Si, Fe, and Mn alloy elements. The content of elements such as Ti and V is about 0.04%.
[0081] (2) Refining and grain refinement: The melt temperature was adjusted to 750°C, and then a high-purity inert gas containing a mixed chloride salt refining agent was introduced into the melt for 10 min; then an Al-B master alloy with a B content of 0.022% was added.
[0082] (3) Composite modification: After standing and keeping warm for 30 minutes, remove the surface scum; then add industrial pure Mg and Al-Sr-RE composite modifier, sprinkle a layer of covering agent on the surface of the melt, and pass preheated inert gas to degas for 5 minutes.
[0083] (4) Casting: After the melt has been allowed to stand for 15 minutes, the dewatering port is opened and the melt is directly supplied to the die-casting equipment or ingot through the flow trough. An online rotary degassing box and a ceramic filter plate can be installed in the flow trough to obtain high-quality castings or ingots.
[0084] Example 4
[0085] A boron-containing die-casting aluminum alloy, comprising the following components in percentage by mass:
[0086] Si 11.0%, Fe 0.65%, Mn 0.15%, Mg 0.18%, B 0.015%, Sr 0.012%, RE 0.04%, the balance is inevitable impurity elements and aluminum. RE is a mixture of La and Ce, and the mass ratio of Ce to La is 2.
[0087] The preparation process of the boron-containing die-casting aluminum alloy is as follows:
[0088] (1) Melting: Add raw materials containing Si, Fe, and Mn into a melting furnace and melt them at 750°C. After the raw materials are melted, take samples to test the alloy composition, and adjust the content of Si, Fe, and Mn alloy elements. The content of elements such as Ti and V is about 0.01%.
[0089] (2) Refining and grain refinement: The melt temperature was adjusted to 730°C, and then a high-purity inert gas containing a mixed chloride salt refining agent was introduced into the melt for 15 min; then an Al-B master alloy with a B content of 0.017% was added.
[0090] (3) Composite modification: After standing and keeping warm for 45 minutes, remove the surface scum; then add industrial pure Mg and Al-Sr-RE composite modifier, sprinkle a layer of covering agent on the surface of the melt, and pass preheated inert gas for degassing for 10 minutes.
[0091] (4) Casting: After the melt is left to stand for 20 minutes, the dewatering port is opened and the melt is directly supplied to the die-casting equipment or ingot through the flow trough. An online rotary degassing box and a ceramic filter plate can be installed in the flow trough to obtain high-quality castings or ingots.
[0092] Comparative Example 1
[0093] A boron-containing die-casting aluminum alloy, which differs from Example 1 in that the composition of Example 1 does not contain the B element; other components and their contents and the preparation process of the alloy are the same as those of Example 1.
[0094] Comparative Example 2
[0095] A boron-containing die-casting aluminum alloy, which differs from Example 2 in that the Fe content of Example 2 is 0.7% and the Mn content is 0.20%; other components and their contents and the preparation process of the alloy are the same as those of Example 2.
[0096] Comparative Example 3
[0097] A boron-containing die-casting aluminum alloy, which differs from Example 3 in that the Mn content of Comparative Example 3 is 0.55%; other components and their contents and the preparation process of the alloy are the same as those of Example 3.
[0098] Comparative Example 4
[0099] A boron-containing die-casting aluminum alloy, which differs from Example 4 in that the composition of Example 4 does not contain RE element; other components and their contents and the preparation process of the alloy are the same as those of Example 4.
[0100] Comparative Example 5
[0101] A boron-containing die-casting aluminum alloy, which differs from Example 1 in that the B content of Comparative Example 5 is 0.005%; other components and their contents and the preparation process of the alloy are the same as those of Example 1.
[0102] Comparative Example 6
[0103] A boron-containing die-casting aluminum alloy, which differs from Example 1 in that Sr in Comparative Example 6 is added in the form of an Al-Sr alloy, and RE is added in the form of an Al-RE alloy; the components and their contents and other preparation processes of the alloy are the same as those in Example 1.
[0104] The alloys of Examples 1 to 4 and Comparative Examples 1 to 6 were selected to prepare die castings, and the castings were divided into two parts, one of which remained in the die-cast state, and the other was subjected to a short-time aging treatment, and the aging treatment process was: 200°C, heat preservation for 40 minutes. The tensile mechanical properties were tested respectively, and the test results were shown in Table 1 according to GB / T 228.1-2021 "Tensile Test of Metallic Materials Part 1: Room Temperature Test Method".
[0105] Table 1 Mechanical properties of the alloys of Examples 1 to 4 and Comparative Examples 1 to 6 in die-cast and aged states
[0106]
[0107]
[0108] Table 1 is analyzed. From the comparison of the die-cast alloys of Examples 1 to 4 and Comparative Examples 1 to 6, it can be seen that the content of Mn and Fe has a greater influence on the plasticity of the alloy. The appropriate Mn and Fe ratio can significantly improve the plasticity of the alloy and increase the strength at the same time. When the alloy contains three elements, namely Sr, RE and B, a die casting with better comprehensive performance can be obtained, and the lack of B or RE will lead to a decrease in the plasticity of the alloy, and will also slightly reduce the tensile strength and yield strength of the casting. It can be seen from Examples 1 to 4 that short-time aging significantly improves the strength and yield strength of the casting, but reduces the plasticity. Therefore, short-time aging is one of the effective methods for regulating the performance of castings.
[0109] The microstructure of the alloy obtained in Example 1 was analyzed in the die-cast state. Figure 1 .Depend on Figure 1 It can be seen that the eutectic silicon grains prepared in Example 1 are evenly distributed, small in size, with an average particle size of about 1.5 μm and high sphericity. Figure 2 This is the tensile curve of the boron-containing die-cast aluminum alloy of Example 1 in the die-cast state, which shows that it has good tensile strength, yield strength and elongation.
[0110] In the embodiment of the present invention, the strength and plasticity of the alloy are mainly achieved by adding strengthening elements and refining the structure. On the one hand, the alloy strength is improved by designing a trace amount of Mg through solid solution strengthening. On the other hand, the grains are refined by B, and the eutectic silicon is deeply modified by Al-Sr-RE to improve the strength of the alloy through grain refinement and second phase refinement. 2 In order to form Si, the Mg content is designed to be at a low level; in order to reduce the loss of B element by V and Ti, the content of V and Ti in the alloy raw materials is considered, and the addition amount of B is appropriately increased; Al-Sr-RE has been proven to have a deep metamorphic effect on eutectic silicon. Fine eutectic silicon can be obtained by adding a trace amount of Al-Sr-RE, which has a significant effect on improving the strength and plasticity of the alloy.
[0111] The boron-containing die-cast aluminum alloy prepared in the embodiment of the present invention has a tensile strength, yield strength and elongation of 290-320 MPa, 130-160 MPa and 15-20% respectively when heat treatment is not required (die-cast state); and after aging treatment (aged state), the tensile strength, yield strength and elongation of the casting reach 300-340 MPa, 160-200 MPa and 13-18% respectively.
[0112] In summary, the present invention is based on the hypoeutectic Al-Si alloy, and carries out alloy composition optimization design and microstructure refinement research. The alloy is endowed with good die-casting performance and plasticity by a specific content of Si. The Fe and Mn contents are regulated on the basis of the Si content, so that the alloy has good demoulding properties and toughness. The solid solution strengthening, grain refinement and second phase refinement are carried out by the action of specific contents of Mg, B and Al-Sr-RE, which effectively improves the strength and plasticity of the alloy. Finally, a high-strength and toughness boron-containing die-casting aluminum alloy is obtained, which has a wide range of applications in automobiles, especially in the field of lightweighting.
Claims
1. A boron-containing die-casting aluminum alloy, It is characterized in that The invention is composed of the following components in mass percentage: 8-11% Si, 0.45-0.65% Fe, 0.15-0.45% Mn, 0.1-0.25% Mg, 0.015-0.025% B, 0.01-0.025% Sr, 0.02-0.05% RE, and the remainder is impurity elements and Al; the sum of the mass percentages of Mn and Fe is 0.7-1.0%; The Sr and RE are added in the form of Al-Sr-RE master alloy.
2. The boron-containing die-casting aluminum alloy according to claim 1, It is characterized in that The RE is a mixture of La and Ce; Preferably, the mass ratio of Ce to La is 2-6.
3. The boron-containing die-casting aluminum alloy according to claim 1, It is characterized in that The impurity elements include one or both of V and Ti or do not include V and Ti.
4. The boron-containing die-casting aluminum alloy according to claim 3, It is characterized in that The composition of the die-cast aluminum alloy has the following relationship: B =0.01%+0.25(W V +W Ti ), W B , W V , W Ti Represent the mass percentages of B, V and Ti respectively.
5. The boron-containing die-casting aluminum alloy according to claim 1, It is characterized in that The properties of the boron-containing die-casting aluminum alloy meet the following conditions: tensile strength is 290-340 MPa; yield strength is 130-200 MPa; elongation is 13-20%; Preferably, the properties of the boron-containing die-cast aluminum alloy meet the following conditions: tensile strength is 300-340 MPa; yield strength is 160-200 MPa; elongation is 13-18%.
6. A method for preparing the boron-containing die-casting aluminum alloy according to any one of claims 1 to 5, It is characterized in that The process comprises the following steps: melting raw materials containing Si, Fe and Mn, adjusting the contents of Si, Fe and Mn to target contents, refining, adjusting the content of B to target content, heat preservation, adjusting the contents of Mg, Sr and RE to target contents, degassing, and casting to obtain the boron-containing die-casting aluminum alloy.
7. The preparation method according to claim 6, It is characterized in that The melting temperature is 750-800°C; And / or, the refining temperature is 720-760°C; And / or, the refining time is 10 to 20 minutes.
8. The preparation method according to claim 6, It is characterized in that The method of regulating the B content is to add Al-B master alloy; And / or, the Mg content is regulated by adding Mg element or Al-Mg master alloy; And / or, the method of adjusting the content of Sr and RE is to add Al-Sr-RE master alloy.
9. The preparation method according to claim 6, It is characterized in that The method further comprises an aging treatment step after casting; the aging treatment temperature is preferably 180 to 220° C.; and the aging treatment time is preferably 30 to 50 minutes.
10. Use of the boron-containing die-casting aluminum alloy according to any one of claims 1 to 5 in the automotive field.
Citation Information
Patent Citations
High-strength high-toughness die-casting aluminum alloy and manufacturing method thereof
CN110157959A
High-strength and high-thermal-conductivity cast aluminum alloy, preparation method thereof and aluminum alloy product
CN114855036A
Eutectic die-casting aluminum alloy material as well as preparation method and application thereof
CN117385239A
Aluminum alloy casting and its manufacturing method
JP2006336044A
Die-cast aluminum alloy material, preparation method therefor, and use thereof
WO2024099374A1