Heat treatment method of 04Cr13Ni5Mo steel large rotating wheel forged piece
Through the heat treatment method of multiple normalization and tempering treatments, the tissue defects of the forgings of large-scale rotors of 04Cr13Ni5Mo steel are solved, which significantly improves its strength and toughness, and is suitable for the high strength and wear resistance requirements of large-scale impact turbine rotors.
Patent Information
- Application Number
- CN202411165923.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-23
AI Technical Summary
04Cr13Ni5Mo steel large-scale rotor forgings are prone to tissue defects during the forging process, which affects their mechanical properties and lacks strength and toughness, making it difficult to meet the requirements of large-scale impact turbine rotors.
Heat treatment methods using multiple normalization and tempering treatments, including the first normalization treatment (1030-1050℃), the second normalization treatment (1010-1020℃), and the third normalization treatment (970-990 ) and multiple tempering treatments, through tissue austenitization, carbide dissolution and microscopic composition homogenization, grain size is refined, and the strength and toughness of the forging are improved.
By refining the grain size and improving the microstructure structure, the strength and toughness of the 04Cr13Ni5Mo steel large-scale rotor forgings are significantly improved, and are suitable for the high strength and wear resistance requirements of large-scale impact turbine rotors.
Smart Images

Figure CN118932144A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heat treatment of steel, and in particular to a heat treatment method for a large 04Cr13Ni5Mo steel runner forging. Background Art
[0002] 04Cr13Ni5Mo steel is a stainless steel with excellent performance, which is suitable for manufacturing the runner of impulse turbine. With the continuous innovation of technology, the original small impulse turbine runner cannot meet the use requirements, so it is necessary to develop a large impulse turbine runner, and then it is necessary to develop 04Cr13Ni5Mo steel large runner forgings. The diameter of the large impulse turbine runner exceeds 4m. During operation, it needs to withstand the impact of ultra-high head water flow and sediment erosion, and drive the generator rotor to operate and generate electricity at a high speed. This requires 04Cr13Ni5Mo steel large runner forgings to have better mechanical properties (strength, toughness, etc.). However, due to the large size and weight of 04Cr13Ni5Mo steel large runner forgings, and the large number of heat treatment processes during the forging process, organizational defects will occur inside the forgings, affecting the mechanical properties of 04Cr13Ni5Mo steel large runner forgings. Therefore, how to improve the mechanical properties of 04Cr13Ni5Mo steel large runner forgings has become an urgent problem to be solved. Summary of the invention
[0003] The problem solved by the invention is how to improve the mechanical properties of a large runner forging made of 04Cr13Ni5Mo steel.
[0004] To solve the above problems, the present invention provides a heat treatment method for a 04Cr13Ni5Mo steel large runner forging, comprising performing post-forging heat treatment and quenching and tempering heat treatment on a forging blank in sequence; wherein the post-forging heat treatment comprises a first normalizing treatment, a second normalizing treatment, a third normalizing treatment and a first tempering treatment in sequence; the quenching and tempering heat treatment comprises a quenching treatment, a second tempering treatment and a third tempering treatment in sequence; the normalizing temperature of the first normalizing treatment is 1030-1050°C, the normalizing temperature of the second normalizing treatment is 1010-1020°C, the normalizing temperature of the third normalizing treatment is 970-990°C, and the tempering temperature of the first tempering treatment is 610-630°C.
[0005] Optionally, the first normalizing treatment includes:
[0006] The forging blank is kept at 640-660° C. for 14-16 hours, heated to 1030-1050° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a first intermediate forging.
[0007] Optionally, the second normalizing treatment includes:
[0008] The first intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 540-560° C., kept for 14-16 hours, then heated to 1010-1020° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a second intermediate forging.
[0009] Optionally, the third normalizing treatment includes:
[0010] The second intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 540-560° C., kept for 9-11 hours, then heated to 970-990° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a third intermediate forging.
[0011] Optionally, the first tempering treatment includes:
[0012] The third intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 610-630° C., kept for 44-46 hours, cooled to 190-200° C. at a cooling rate of 9-11° C. / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
[0013] Optionally, the quenching treatment includes:
[0014] The fourth intermediate forging is heated to 980-1020° C. for 16-22 hours, and cooled to 130-160° C. by blasting to obtain a fifth intermediate forging.
[0015] Optionally, the second tempering treatment includes:
[0016] The fifth intermediate forging is heated to 560-600° C., kept at this temperature for 22-36 hours, and air-cooled to 130-160° C. to obtain a sixth intermediate forging.
[0017] Optionally, the third tempering treatment includes:
[0018] The sixth intermediate forging is heated to 580-610° C., kept at the temperature for 28-44 hours, and then taken out of the furnace and cooled to obtain a large runner forging.
[0019] Optionally, the diameter of the forging blank is greater than 4 m.
[0020] Optionally, the components of the forging blank include, by weight percentage: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.0%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the remainder is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.
[0021] Compared with the prior art, the heat treatment method for large runner forgings provided by the present invention can make the structure in the forging fully austenitized by controlling the normalizing temperature of the first normalizing treatment to 1030-1050°C, and can ensure that part of the carbides are fully dissolved, so that some micro-segregated elements undergo short-range diffusion, and achieve uniformity of micro-components, which is beneficial to improving the strength and toughness of large runner forgings; by controlling the normalizing temperature of the second normalizing treatment to 1010-1020°C, so that the normalizing temperature of the second normalizing treatment is slightly lower than the normalizing temperature of the first normalizing treatment, it can ensure further refinement of the grain size of the forging, and can make part of the carbides By controlling the normalizing temperature of the third normalizing treatment to 970-990°C, the normalizing temperature of the third normalizing treatment is further reduced, so that some fine carbides are dispersed in the austenite, which plays a role in pinning the grain boundaries, thereby further refining the grain size of the forging, which is conducive to further improving the strength and toughness of the large runner forging; by controlling the tempering temperature of the first tempering treatment to 610-630°C, the structure in the forging undergoes an inverse austenite transformation, which can effectively improve the toughness of the forging, and is conducive to reducing the hardness of the forging, which is convenient for later rough processing. In summary, the large runner forging obtained by the heat treatment method of the large runner forging provided by the present invention has a finer grain size, better strength and better toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a metallographic structure picture of the large runner forging prepared in Example 1;
[0023] Figure 2 This is a metallographic structure picture of the large runner forging prepared in Example 2;
[0024] Figure 3 This is a metallographic structure picture of the large runner forging prepared in Example 3;
[0025] Figure 4 This is a metallographic structure picture of the large runner forging prepared in Comparative Example 1;
[0026] Figure 5 This is a metallographic structure picture of the large runner forging prepared in Comparative Example 2. DETAILED DESCRIPTION
[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0029] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0030] It should be noted that the 04Cr13Ni5Mo steel large runner forging in the present invention refers to a 04Cr13Ni5Mo steel runner forging with a diameter exceeding 4m.
[0031] A heat treatment method for a 04Cr13Ni5Mo steel large runner forging provided in an embodiment of the present invention comprises performing post-forging heat treatment and quenching and tempering heat treatment on a forging blank in sequence; wherein the post-forging heat treatment comprises a first normalizing treatment, a second normalizing treatment, a third normalizing treatment and a first tempering treatment in sequence; the quenching and tempering heat treatment comprises a quenching treatment, a second tempering treatment and a third tempering treatment in sequence; the normalizing temperature of the first normalizing treatment is 1030-1050°C, the normalizing temperature of the second normalizing treatment is 1010-1020°C, the normalizing temperature of the third normalizing treatment is 970-990°C, and the tempering temperature of the first tempering treatment is 610-630°C.
[0032] The heat treatment method for large runner forgings provided by the embodiment of the present invention can make the structure in the forging fully austenitized by controlling the normalizing temperature of the first normalizing treatment to 1030-1050°C, and can ensure that part of the carbides are fully dissolved, so that some micro-segregated elements undergo short-range diffusion, and achieve uniformity of micro-components, which is beneficial to improving the strength and toughness of the large runner forgings; by controlling the normalizing temperature of the second normalizing treatment to 1010-1020°C, so that the normalizing temperature of the second normalizing treatment is slightly lower than the normalizing temperature of the first normalizing treatment, it can ensure further refinement of the grain size of the forging, and can make part of the carbides melt into the austenite. By controlling the normalizing temperature of the third normalizing treatment to 970-990°C, the normalizing temperature of the third normalizing treatment is further reduced, so that some fine carbides are dispersed in the austenite, which plays a role in fixing the grain boundaries, thereby further refining the grain size of the forging, which is beneficial to further improve the strength and toughness of the large runner forging; by controlling the tempering temperature of the first tempering treatment to 610-630°C, the structure in the forging undergoes reverse austenite transformation, which can effectively improve the toughness of the forging, and is beneficial to reduce the hardness of the forging, which is convenient for later rough processing. In summary, the large runner forging obtained by the heat treatment method for large runner forgings provided by the embodiment of the present invention has a finer grain size, better strength and better toughness.
[0033] It should be noted that the forging blank in the embodiment of the present invention is forged from 04Cr13Ni5Mo steel ingot, the initial forging temperature during the forging process is 1180°C, and the final forging temperature is 850°C.
[0034] In some embodiments of the present invention, the first normalizing treatment comprises:
[0035] The forging blank is kept at 640-660° C. for 14-16 hours, heated to 1030-1050° C. at a rate of 40-60° C. / h, kept at this temperature for 35-37 hours, and air-cooled to 130-160° C. to obtain a first intermediate forging.
[0036] In this embodiment, the forging blank is kept at 640-660°C for 14-16h to avoid cracking of the forging blank due to excessively low temperature during operation; the temperature is raised to 1030-1050°C at a rate of 40-60°C / h to ensure recrystallization of the forging.
[0037] In some embodiments of the present invention, the second normalizing treatment comprises:
[0038] The first intermediate forging is kept at 130-160°C for 19-21h, heated to 540-560°C at a rate of 20-40°C / h, kept for 14-16h, then heated to 1010-1020°C at a rate of 40-60°C / h, kept for 35-37h, and air-cooled to 130-160°C to obtain a second intermediate forging.
[0039] In this embodiment, the first intermediate forging is kept at 130-160°C for 19-21h, which can ensure sufficient transformation of the core structure of the forging, reduce the residual austenite content, and is beneficial to further improve the strength of the forging; the temperature is raised to 540-560°C at a relatively slow rate (20-40°C / h) and kept for 14-16h, which can effectively prevent excessive thermal stress in the forging; the temperature is raised to 1010-1020°C at a relatively fast rate (40-60°C / h), which can effectively increase the nucleation speed of the material and increase the number of nucleations per unit volume, which is beneficial to further refine the grains.
[0040] In some embodiments of the present invention, the third normalizing treatment comprises:
[0041] The second intermediate forging is kept at 130-160°C for 19-21h, heated to 540-560°C at a rate of 20-40°C / h, kept for 9-11h, then heated to 970-990°C at a rate of 40-60°C / h, kept for 35-37h, and air-cooled to 130-160°C to obtain a third intermediate forging.
[0042] In this embodiment, the second intermediate forging is kept at 130-160°C for 19-21h, which can ensure sufficient transformation of the core structure of the forging and reduce the residual austenite content, which is beneficial to further improve the strength of the forging; the temperature is raised to 540-560°C at a relatively slow rate (20-40°C / h) and kept for 9-11h, which can effectively prevent excessive thermal stress in the forging; the temperature is raised to 970-990°C at a relatively fast rate (40-60°C / h), which can effectively increase the nucleation speed of the material and increase the number of nucleations per unit volume, which is beneficial to further refine the grains.
[0043] In some embodiments of the present invention, the first tempering treatment includes:
[0044] The third intermediate forging is kept at 130-160°C for 19-21h, heated to 610-630°C at a rate of 30-40°C / h, kept for 44-46h, cooled to 190-200°C at a cooling rate of 9-11°C / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
[0045] In this embodiment, the third intermediate forging is kept at 130-160°C for 19-21 hours, which can ensure sufficient transformation of the core structure of the forging and reduce the residual austenite content, which is beneficial to further improve the strength of the forging; heating to 610-630°C at a relatively slow rate (30-40°C / h) and keeping it for 44-46 hours can effectively prevent excessive thermal stress in the forging.
[0046] In some embodiments of the present invention, the quenching treatment comprises:
[0047] The fourth intermediate forging is heated to 980-1020° C. for 16-22 hours, and cooled to 130-160° C. by blasting to obtain a fifth intermediate forging.
[0048] In some embodiments of the present invention, the second tempering treatment includes:
[0049] The fifth intermediate forging is heated to 560-600° C., kept at this temperature for 22-36 hours, and air-cooled to 130-160° C. to obtain a sixth intermediate forging.
[0050] In some embodiments of the present invention, the third tempering treatment includes:
[0051] The sixth intermediate forging is heated to 580-610° C., kept at the temperature for 28-44 hours, and then taken out of the furnace and cooled to obtain a large runner forging.
[0052] In some embodiments of the present invention, the diameter of the forging blank is greater than 4 m.
[0053] In some embodiments of the present invention, the components of the forging blank include, by weight percentage: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.0%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the remainder is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.
[0054] The present invention is further described below in conjunction with specific embodiments.
[0055] Example 1
[0056] A1. First normalizing treatment: keep the forging blank at 650°C for 15h, heat it to 1040°C at a rate of 50°C / h, keep it for 36h, and air-cool it to 145°C to obtain a first intermediate forging; wherein the diameter of the forging blank is 4900mm and the height is 1120mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.
[0057] A2. Second normalizing treatment: the first intermediate forging is kept at 145°C for 20 hours, heated to 550°C at a rate of 30°C / h, kept for 15 hours, then heated to 1020°C at a rate of 50°C / h, kept for 36 hours, and air-cooled to 145°C to obtain a second intermediate forging.
[0058] A3. Third normalizing treatment: keep the second intermediate forging at 145°C for 20 hours, heat it to 550°C at a rate of 30°C / h, keep it for 10 hours, then heat it to 980°C at a rate of 50°C / h, keep it for 36 hours, and air-cool it to 145°C to obtain the third intermediate forging.
[0059] A4. First tempering treatment: the third intermediate forging is kept at 145°C for 20 hours, heated to 620°C at a rate of 35°C / h, kept at this temperature for 45 hours, cooled to 200°C at a rate of 10°C / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
[0060] A5. Quenching treatment: the fourth intermediate forging is heated to 1000° C. and kept at this temperature for 19 hours, and then cooled to 145° C. by blasting to obtain a fifth intermediate forging.
[0061] A6. Second tempering treatment: the fifth intermediate forging is heated to 580° C., kept at this temperature for 29 hours, and air-cooled to 145° C. to obtain a sixth intermediate forging.
[0062] A7. Third tempering treatment: The sixth intermediate forging is heated to 600° C. and kept at this temperature for 36 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.
[0063] Example 2
[0064] A1. First normalizing treatment: keep the forging blank at 640°C for 16 hours, heat it to 1030°C at a rate of 40°C / h, keep it for 37 hours, and air-cool it to 130°C to obtain a first intermediate forging; wherein the diameter of the forging blank is 4600 mm and the height is 1120 mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.
[0065] A2. Second normalizing treatment: the first intermediate forging is kept at 130°C for 21 hours, heated to 540°C at a rate of 20°C / h, kept for 16 hours, then heated to 1010°C at a rate of 40°C / h, kept for 37 hours, and air-cooled to 130°C to obtain a second intermediate forging.
[0066] A3. Third normalizing treatment: keep the second intermediate forging at 130°C for 21 hours, heat it to 540°C at a rate of 20°C / h, keep it for 11 hours, then heat it to 970°C at a rate of 40°C / h, keep it for 37 hours, and air-cool it to 130°C to obtain the third intermediate forging.
[0067] A4. First tempering treatment: the third intermediate forging is kept at 130°C for 21 hours, heated to 610°C at a rate of 30°C / h, kept for 46 hours, cooled to 190°C at a rate of 9°C / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
[0068] A5. Quenching treatment: The fourth intermediate forging is heated to 980° C. and kept at this temperature for 22 hours, and then cooled to 130° C. by blasting to obtain a fifth intermediate forging.
[0069] A6. Second tempering treatment: the fifth intermediate forging is heated to 560° C., kept at this temperature for 36 hours, and air-cooled to 130° C. to obtain a sixth intermediate forging.
[0070] A7. Third tempering treatment: The sixth intermediate forging is heated to 580° C. and kept at this temperature for 44 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.
[0071] Example 3
[0072] A1. First normalizing treatment: keep the forging blank at 660°C for 14h, heat it to 1050°C at a rate of 60°C / h, keep it for 35h, and air-cool it to 160°C to obtain a first intermediate forging; wherein the diameter of the forging blank is 4200mm and the height is 1120mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.
[0073] A2. Second normalizing treatment: the first intermediate forging is kept at 160°C for 19 hours, heated to 560°C at a rate of 40°C / h, kept at this temperature for 14 hours, then heated to 1020°C at a rate of 60°C / h, kept at this temperature for 35 hours, and air-cooled to 160°C to obtain a second intermediate forging.
[0074] A3. Third normalizing treatment: keep the second intermediate forging at 160°C for 19 hours, heat it to 560°C at a rate of 40°C / h, keep it for 9 hours, then heat it to 990°C at a rate of 60°C / h, keep it for 35 hours, and air-cool it to 160°C to obtain the third intermediate forging.
[0075] A4. First tempering treatment: the third intermediate forging is kept at 160°C for 19 hours, heated to 630°C at a rate of 40°C / h, kept at this temperature for 44 hours, cooled to 200°C at a rate of 11°C / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
[0076] A5. Quenching treatment: The fourth intermediate forging is heated to 1020° C. and kept at this temperature for 16 hours, and then cooled to 160° C. by blasting to obtain a fifth intermediate forging.
[0077] A6. Second tempering treatment: heat the fifth intermediate forging to 580° C., keep the temperature for 22 h, and air cool to 160° C. to obtain a sixth intermediate forging.
[0078] A7. Third tempering treatment: The sixth intermediate forging is heated to 610° C. and kept at this temperature for 28 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.
[0079] Comparative Example 1
[0080] B1. Annealing and isothermal treatment: keep the forging blank at 650°C for 20h, heat it to 1040°C at a rate of 45°C / h, keep it for 36h, furnace cool it to 560°C, keep it for 240h, furnace cool it to 200°C, and cool it to room temperature to obtain a first intermediate forging; wherein the diameter of the forging blank is 4900mm and the height is 1120mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.
[0081] B2. Quenching treatment: the first intermediate forging is heated to 1000° C. for 19 hours, and cooled to 145° C. by blasting to obtain a second intermediate forging.
[0082] B3. Primary tempering treatment: the second intermediate forging is heated to 580° C., kept at this temperature for 29 h, and air-cooled to 145° C. to obtain a third intermediate forging.
[0083] B4. Secondary tempering treatment: The third intermediate forging is heated to 600° C. and kept at this temperature for 36 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.
[0084] Comparative Example 2
[0085] B1. Annealing and isothermal treatment: the forging blank is kept at 650°C for 20 hours, heated to 1040°C at a rate of 45°C / h, kept for 36 hours, furnace cooled to 560°C, kept for 240 hours, furnace cooled to 200°C, and cooled to room temperature to obtain a first intermediate forging; the first intermediate forging is heated to 650°C, kept for 20 hours, heated to 990°C at a rate of 45°C / h, kept for 36 hours, furnace cooled to 560°C, kept for 240 hours, furnace cooled to 200°C, and cooled to room temperature. A second intermediate forging is obtained; wherein, the diameter of the forging blank is 4900 mm and the height is 1120 mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.
[0086] B2. Quenching treatment: the second intermediate forging is heated to 1000° C., kept at this temperature for 19 hours, and cooled to 145° C. by blasting to obtain a third intermediate forging.
[0087] B3. Primary tempering treatment: heating the third intermediate forging to 580° C., keeping the temperature for 29 hours, and air cooling to 145° C. to obtain a fourth intermediate forging.
[0088] B4. Secondary tempering treatment: The fourth intermediate forging is heated to 600° C. and kept at this temperature for 36 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.
[0089] Example
[0090] The metallographic structures of the large runner forgings prepared in Examples 1-3 and Comparative Examples 1-2 were characterized. Figure 1-5 ,from Figure 1-5 It can be seen that the grain sizes of the large runner forgings prepared in Examples 1-3 and Comparative Examples 1-2 are 2.8, 3.3, 4.3, 1.0 and 1.3, respectively, and the mixed crystals in the large runner forgings prepared in Comparative Examples 1-2 are relatively serious. It can be seen that the grain size of the large runner forgings prepared in Examples 1-3 is finer than that in Comparative Examples 1-2. It should be noted that the higher the grain size grade, the finer the grain size.
[0091] The mechanical properties and flaw detection limit sensitivity of the large runner forgings prepared in Examples 1-3 and Comparative Examples 1-2 were characterized, and the results are shown in Table 1. It can be seen from Table 1 that, compared with Comparative Examples 1-2, the yield strength, tensile strength, cross-sectional shrinkage rate and AKv of the large forgings in Examples 1-3 are higher, indicating that the large forgings in Examples 1-3 have higher strength and toughness; it can be seen from Table 1 that, compared with Comparative Examples 1-2, the flaw detection limit sensitivity of the large forgings in Examples 1-3 is higher.
[0092] Table 1
[0093]
[0094] It should be noted that the radial and axial directions in Table 1 correspond to the radial and axial properties of the forgings respectively, Rp0.2 represents the yield strength, Rm represents the tensile strength, AKv is used to characterize the impact toughness, representing the energy absorbed by the material when subjected to an impact load, A represents the elongation after fracture, and Z represents the reduction of area.
[0095] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A heat treatment method for a large 04Cr13Ni5Mo steel runner forging, characterized in that: The method comprises performing post-forging heat treatment and quenching and tempering heat treatment on the forging blank in sequence; wherein the post-forging heat treatment comprises a first normalizing treatment, a second normalizing treatment, a third normalizing treatment and a first tempering treatment in sequence; the quenching and tempering heat treatment comprises a quenching treatment, a second tempering treatment and a third tempering treatment in sequence; the normalizing temperature of the first normalizing treatment is 1030-1050°C, the normalizing temperature of the second normalizing treatment is 1010-1020°C, the normalizing temperature of the third normalizing treatment is 970-990°C, and the tempering temperature of the first tempering treatment is 610-630°C.
2. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 1, characterized in that: The first normalizing treatment comprises: The forging blank is kept at 640-660° C. for 14-16 hours, heated to 1030-1050° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a first intermediate forging.
3. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 2, characterized in that: The second normalizing treatment comprises: The first intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 540-560° C., kept for 14-16 hours, then heated to 1010-1020° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a second intermediate forging.
4. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 3, characterized in that: The third normalizing treatment comprises: The second intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 540-560° C., kept for 9-11 hours, then heated to 970-990° C., kept for 35-37 hours, and air-cooled to 130-160° C. to obtain a third intermediate forging.
5. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 4, characterized in that: The first tempering treatment comprises: The third intermediate forging is kept at 130-160° C. for 19-21 hours, heated to 610-630° C., kept for 44-46 hours, cooled to 190-200° C. at a cooling rate of 9-11° C. / h, and air-cooled to room temperature to obtain a fourth intermediate forging.
6. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 5, characterized in that: The quenching treatment comprises: The fourth intermediate forging is heated to 980-1020° C. for 16-22 hours, and cooled to 130-160° C. by blasting to obtain a fifth intermediate forging.
7. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 6, characterized in that: The second tempering treatment comprises: The fifth intermediate forging is heated to 560-600° C., kept at this temperature for 22-36 hours, and air-cooled to 130-160° C. to obtain a sixth intermediate forging.
8. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 7, characterized in that: The third tempering treatment comprises: The sixth intermediate forging is heated to 580-610° C., kept at the temperature for 28-44 hours, and then taken out of the furnace and cooled to obtain a large runner forging.
9. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 1, characterized in that: The diameter of the forging blank is more than 4m.
10. The heat treatment method of 04Cr13Ni5Mo steel large runner forging according to claim 1, characterized in that: Measured by weight percentage, the components of the forging blank include: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.0%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the balance is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.
Citation Information
Patent Citations
Heat treatment method of 30GrNi3MoV forged pieces
CN103320591A
Heat treatment method for strength of 28CrMoNiV steel capable of improving industrial steam turbine rotor forge piece
CN104946870A
Annealing process of 04Cr13Ni5Mo super martensitic stainless steel medium plate for water and electricity
CN112430714A
Heat treatment method for oversized 0Cr13Ni5Mo martensitic stainless steel forgings
CN117165746A
Process for producing high-and low-pressure integral-type turbine rotor
US5716468A
Cited By
Post-forging heat treatment method and auxiliary tool for fountain forge piece
CN119553057A
Manufacturing method of mushroom head forge piece of miter gate bottom pivot of ship lock of large hydropower station
CN121592836A
Heat treatment method for large 04cr13ni5mo steel runner forged piece
WO2026041154A1
Post-forging heat treatment method for runner bucket forging, and auxiliary tool
WO2026118610A1