Antibacterial polyether-ether-ketone / polyphenyl sulfone triple shape memory composite material

By using antibacterial polyetheretherketone/polyphenylsulfone triple shape memory composites in shape memory composites, combined with the ratio control of PEEK, PPSU and zeolite antibacterial agents, the problems of existing materials in terms of biocompatibility and deformation recovery are solved. restriction, achieving triple shape memory and high antibacterial effect, expanding its application scope.

CN118756374AActive Publication Date: 2024-10-11常州君华医疗科技有限公司 +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411021253.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-11
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing shape memory composite materials have limitations in biocompatibility, deformation recovery, driving speed and fatigue life, and most of them have single or dual shape memory effects, which cannot meet the needs of complex applications, especially the demand for antibacterial materials in the medical field. growing day by day.

Method used

Develop antibacterial polyetheretherketone/polyphenylsulfone triple shape memory composite materials. By mixing PEEK and PPSU in a specific ratio, adding antibacterial ions using zeolite as a carrier to prepare antibacterial agents, and producing a fibrous composite through a melt spinning cooling process. material, achieving triple shape memory effect and high antibacterial rate.

Benefits of technology

It achieves the material's triple shape memory effect and high antibacterial rate, broadens its application potential in biomedical, aerospace and smart wearable fields, reduces the risk of infection, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967330340000061
    Figure BDA0004967330340000061
  • Figure BDA0004967330340000062
    Figure BDA0004967330340000062
  • Figure BDA0004967330340000071
    Figure BDA0004967330340000071
Patent Text Reader

Abstract

The invention relates to the technical field of shape memory composite materials, in particular to an antibacterial polyether-ether-ketone / polyphenyl sulfone triple shape memory composite material which comprises resin and an antibacterial agent. The resin is composed of PEEK and PPSU according to a mass ratio of 70: 30 to 50: 50; the preparation method comprises the following steps: uniformly mixing PEEK and PPSU to form a melt blending system, adding an antibacterial agent into the melt blending system, carrying out melt spinning, and carrying out strand cooling and curing to obtain the fibrous antibacterial polyether-ether-ketone / polyphenyl sulfone triple shape memory composite material. By designing and adjusting the proportion of the PEEK, the PPSU and the antibacterial agent, the prepared composite material has a good triple shape memory effect, the shape memory temperature and the antibacterial effect can be regulated and controlled according to the proportion of the PEEK, the PPSU and the antibacterial agent, and the composite material can respond to different temperature stimuli and restore to an initial shape from a plurality of preset temporary shapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shape memory composite materials, in particular to an antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material. Background Art

[0002] Shape memory composites are smart materials that can change shape under certain conditions and return to their original shape afterwards. Such materials usually consist of a stationary phase and a reversible phase, which are cross-linked to form an interpenetrating polymer network structure. The stationary phase is mainly responsible for memorizing the original shape of the material and can be a chemical cross-linking point (thermosetting) or a physical cross-linking point (thermoplastic). The reversible phase has the ability to deform and can be in a crystalline or amorphous state. Its transition temperature (T trans ) can be the melting temperature (T m ) or glass transition temperature (T g ), which enables the material to undergo a phase change at a specific temperature, thereby triggering the shape memory effect.

[0003] Shape memory composites are widely used in many fields, including aerospace, biomedicine, electronics, smart textiles and self-assembly technology. For example, in the aerospace field, they are used to make complex structural parts; in the biomedical field, they are used to make surgical sutures and vascular stents; in electronics, they are used to make flexible connecting parts.

[0004] Although shape memory composites have a wide range of application potential, they also face some technical challenges. For example, shape memory alloys have limitations in biocompatibility, deformation recovery, actuation speed and fatigue life. In addition, existing shape memory materials often only have single or dual shape memory effects, which limits their use in complex applications. In addition, there is a growing demand for materials with antibacterial properties in the medical field to reduce the risk of postoperative infection. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material. The composite material of the present invention not only has good antibacterial properties, but also has good triple shape memory effect.

[0006] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0007] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and an antibacterial agent in a range of 0% to 30% by mass of the resin;

[0008] The resin is composed of PEEK and PPSU in a mass ratio of 70:30 to 40:60. For example, typical ratios of PEEK and PPSU include 70:30, 60:40, 50:50, and 40:60.

[0009] The preparation method thereof comprises the following steps:

[0010] PEEK and PPSU are uniformly mixed to form a melt blend system, an antibacterial agent is added thereto, and the mixture is first melt-spun and then cooled and solidified to obtain a fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material.

[0011] Furthermore, the antibacterial agent uses zeolite as a carrier and loads antibacterial ions; the antibacterial ions are selected from one or more of silver ions, zinc ions, zirconium ions, and copper ions; the configuration of the zeolite is selected from clinoptilolite or type A zeolite; the particle size of the zeolite is 100-200 μm; the loading mass percentage of the antibacterial ions in the antibacterial agent is 0.5-1%.

[0012] Furthermore, the preparation method of the antibacterial agent includes the following steps: placing zeolite in an aqueous solution of nitrate, heating and mixing the reaction under dark conditions, maintaining the pH value of the system between 6 and 8 during this period, separating the solid and the liquid, washing and drying for multiple times, and then roasting.

[0013] Preferably, the nitrate is selected from one or more of silver nitrate, zinc nitrate, zirconium nitrate and copper nitrate, and the molar concentration of the aqueous solution of the nitrate is in the range of 0.1-0.5 mol / L.

[0014] Preferably, the temperature of the heating mixing reaction is 50-70° C. and the reaction time is 3-5 hours; the temperature of the roasting is 350-420° C. and the time is 40-80 minutes.

[0015] Furthermore, the antibacterial agent accounts for 5%-25% of the mass of the resin.

[0016] Furthermore, the melt blending system is formed by a screw extruder, the melt blending temperature is 250-280°C, and the antibacterial agent is added at the side feeding port of the screw extruder; the fiber diameter of the fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is 200-500μm; the filament cooling and solidification adopts multiple cooling rollers to cool the spinning, and the temperature of the cooling roller is lower than the long-term use temperature of PPSU, such as the cooling roller temperature is set between 180°C and 200°C.

[0017] Beneficial technical effects:

[0018] The present invention makes the composite material have a good triple shape memory effect by adjusting the ratio between PEEK, PPSU and the zeolite antibacterial agent loaded with antibacterial ions. The ratio between the three can regulate the response temperature and antibacterial effect of the shape memory effect, so that the composite material can respond to different temperature stimuli and recover from multiple preset temporary shapes to the initial shape.

[0019] The present invention selects corresponding zeolites with good heat resistance as carriers of antibacterial ions, with an antibacterial rate of up to 96%, which is particularly suitable for use in the medical field and can reduce the risk of infection; the composite material of the present invention greatly broadens its application potential in the fields of biomedicine, aerospace, smart wearables, etc.; the preparation method of the present invention is simple and easy to mass produce. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0022] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, the method is carried out in accordance with the general standard requirements or general methods.

[0023] Example 1

[0024] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material, comprising 100 parts by mass of a resin; the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0025] The preparation method thereof comprises the following steps:

[0026] PEEK and PPSU are mixed evenly according to a ratio and added into a twin-screw extruder to form a melt blending system at 250°C. After melt spinning and filament cooling and solidification, a fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is obtained with a fiber diameter of 200-500μm.

[0027] Example 2

[0028] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material, comprising 100 parts by mass of a resin and a silver-loaded clinoptilolite antibacterial agent accounting for 5% by mass of the resin; the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0029] The preparation method thereof comprises the following steps:

[0030] PEEK and PPSU are mixed evenly according to a ratio and added to a twin-screw extruder to form a melt blending system at 250°C. At the same time, a silver-loaded clinoptilolite antibacterial agent is added to the side feed port of the twin-screw extruder for melt blending. After melt spinning and filament cooling and solidification, a fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is obtained with a fiber diameter of 200-500μm.

[0031] The preparation method of the silver-loaded clinoptilolite antibacterial agent in this case is as follows: 10 g of clinoptilolite powder (powder particle size 100-200 μm) is added to 100 mL of 0.1 mol / L AgNO3 solution, and a heating and mixing reaction is carried out in the dark. The temperature of the heating and mixing reaction is 60°C, and the mixing time lasts for 4 hours. During this period, dilute nitric acid (0.1 mol / L) is used to maintain the pH value of the solution between 6 and 8. After the reaction is completed, vacuum filtration is performed for solid-liquid separation, and the separated solid sample is redispersed in 100 mL of distilled water for washing to remove possible residues. After repeated washing and filtration steps, the sample is ensured to be clean, and dried at 90°C for 12 hours to remove moisture; the dried sample is then placed in a muffle furnace, heated from room temperature to 400°C at a rate of 10°C / min, and calcined at the final temperature for 1 hour, and cooled naturally to finally obtain silver-loaded clinoptilolite, and the mass percentage of silver loaded in the antibacterial agent is about 0.5-0.8%, and the silver content decreases slightly after calcination.

[0032] Example 3

[0033] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 10% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0034] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as in Example 2.

[0035] Example 4

[0036] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin composition is: the mass ratio of PEEK to PPSU is 60:40.

[0037] Example 5

[0038] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin composition is: the mass ratio of PEEK to PPSU is 50:50.

[0039] Example 6

[0040] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin composition is: the mass ratio of PEEK to PPSU is 40:60.

[0041] Example 7

[0042] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 15% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0043] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as in Example 2.

[0044] Example 8

[0045] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 20% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0046] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as in Example 2.

[0047] Example 9

[0048] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 25% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 70:30;

[0049] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as in Example 2.

[0050] Example 10

[0051] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 20% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 60:40;

[0052] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as that in Example 2, except that the temperature of the melt blending is 280°C.

[0053] Embodiment 11

[0054] An antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material comprises 100 parts by mass of a resin and 20% by mass of silver-loaded clinoptilolite (same as in Example 2); the resin is composed of PEEK and PPSU, and the mass ratio of PEEK to PPSU is 50:50;

[0055] The preparation of the antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is the same as that in Example 2, except that the temperature of the melt blending is 280°C.

[0056] Comparative Example 1

[0057] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin is only PEEK.

[0058] Comparative Example 2

[0059] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin is only PPSU.

[0060] Comparative Example 3

[0061] The preparation process of the composite material in this case is the same as that of Example 2, except that the resin composition is: the mass ratio of PEEK to PPSU is 80:20.

[0062] Comparative Example 4

[0063] The preparation process of the composite material in this case is the same as that of Example 2, except that zeolite loading is not used, and nanosilver is directly added at the side feed port, and other operations are the same as those of Example 2. The proportion of nanosilver in the composite material is 1%.

[0064] Test Case

[0065] The composite materials of the above cases were molded (molding temperature 400-420°C, molding pressure 100-150MPa, molding time 1min) to obtain a spline (speline size 50mm×3mm×1mm), and a shape memory test was performed on it. The test method is as follows:

[0066] First, prepare two "straight strip" samples (this is the permanent shape S0) at the programming temperature T prog1 (240℃) and deformed under external force, cooled to T prog2 (150°C), remove the external force and obtain the "JL" shape (this is the first temporary shape S1);

[0067] Then, it is further deformed at 150°C and under the action of external force and cooled to 25°C, and the external force is removed to obtain a "70" shape (this is the second temporary shape S2);

[0068] Finally, the sample was heated to 150℃ and 240℃ in turn, and the shape recovery time of the spline shape from the second temporary shape "7 0" to the first temporary shape "JL" and the permanent shape "straight strip" was investigated. The driving force for the spline shape recovery is provided by the entropy elasticity of the molecular chain segments.

[0069] The shape fixation rate and shape recovery rate of the material were tested using the Q800 dynamic thermomechanical analyzer produced by TA Instruments, USA.

[0070] The triple shape memory test method is as follows: (i) The sample is heated to a first programming temperature T prog1 (T g1 +10℃) and force, from the initial shape (ε S0 ) stretched to 5% deformation (ε S1,load );(ii) cooling to the second programming temperature T prog2 (T g2 +10℃, remove the force and obtain the first temporary shape (ε S1 ); (iii) in T prog2 The sample was stretched to 10% deformation (ε S2,load ); (iv) cooling to 25°C, removing the force, and obtaining the second temporary shape (ε S2 ); (v) In the shape recovery stage, the temperature is raised to T prog2 , the shape is restored to ε S1,rec (vi) Heating to T prog1 , the deformation returns to ε S0,rec . Triple shape memory R f and R r Calculated by formulas (1-1), (1-2), (1-3) and (1-4).

[0071]

[0072] See Tables 1 and 2 for data.

[0073] Table 1 Performance of each embodiment

[0074]

[0075]

[0076] Table 2 Performance of the embodiments and their comparative examples

[0077]

[0078] As shown in Tables 1 and 2, the antibacterial composite material of the present invention has a good triple shape memory effect by designing and adjusting the ratio of PEEK, PPSU and the antibacterial agent, and has good shape fixing effect and shape recovery effect, and a short shape recovery time. However, the antibacterial composite material made of only polyetheretherketone or polyphenylsulfone does not have the triple shape memory effect.

[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. Antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material, characterized in that: The invention comprises 100 parts by mass of a resin and an antibacterial agent in an amount ranging from 0% to 30% by mass of the resin; The resin is composed of PEEK and PPSU in a mass ratio of 70:30 to 40:60; The preparation method thereof comprises the following steps: PEEK and PPSU are uniformly mixed to form a melt blend system, an antibacterial agent is added thereto, and the mixture is first melt-spun and then cooled and solidified to obtain a fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material.

2. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to claim 1, characterized in that: The antibacterial agent uses zeolite as a carrier and carries antibacterial ions; The antibacterial ions are selected from one or more of silver ions, zinc ions, zirconium ions, and copper ions. The configuration of the zeolite is selected from clinoptilolite or type A zeolite. The particle size of the zeolite is 100-200 μm. The loading mass percentage of the antibacterial ions in the antibacterial agent is 0.5-1%.

3. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to claim 2, characterized in that: The preparation method of the antibacterial agent comprises the following steps: The zeolite is placed in a nitrate aqueous solution and heated and mixed for reaction in the dark, during which the pH value of the system is maintained between 6 and 8, and the solid and liquid are separated, washed and dried for multiple times, and then roasted.

4. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to claim 3, characterized in that: The nitrate is selected from one or more of silver nitrate, zinc nitrate, zirconium nitrate and copper nitrate, and the molar concentration of the aqueous solution of the nitrate is in the range of 0.1-0.5 mol / L.

5. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to claim 3, characterized in that: The temperature of the heating mixing reaction is 50-70° C. and the reaction time is 3-5 hours; the temperature of the roasting is 350-420° C. and the time is 40-80 minutes.

6. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to any one of claims 1 to 5, characterized in that: The antibacterial agent accounts for 5%-25% of the resin mass.

7. The antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material according to claim 6, characterized in that: The melt blending system is formed by a screw extruder, the melt blending temperature is 250-280° C., and the antibacterial agent is added at the side feeding port of the screw extruder; The fiber diameter of the fibrous antibacterial polyetheretherketone / polyphenylsulfone triple shape memory composite material is 200-500 μm; The filaments are cooled and solidified by using a plurality of cooling rollers for spinning cooling, and the temperature of the cooling rollers is lower than the long-term use temperature of PPSU.

Citation Information

Patent Citations

  • Improved fabrics

    CN101680125A

  • Method for manufacturing a three-dimensional object using PAEK and paes

    CN110268002A

  • High flow polymer compositions

    CN110914337A

  • Method for manufacturing a three-dimensional object using paek and paes

    CN111777848A

  • Antiviral polypropylene non-woven fabric and preparation method thereof

    CN113337903A