Low-temperature crystallized alumina fiber and preparation method thereof
By using the electrospinning method of spinning aids and additives in the preparation of alumina fibers, the problems of complex preparation of alumina fibers and high crystallization temperature are solved, and the preparation of low-temperature crystallized alumina fibers with a simple production cycle and a small fiber diameter is achieved And the surface is smooth.
Patent Information
- Application Number
- CN202410742650.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
AI Technical Summary
The existing alumina fiber preparation methods are complex, the production cycle is long, the fiber diameter is large, the surface is not smooth, and the alumina is difficult to crystallize at low temperatures.
Spinning aids, aluminum salts and additives are stirred in an alcohol solution to form a spinning liquid. Precursor fibers are obtained through electrospinning, pre-oxidized and heat treated, and the spinning environment and conditions are controlled to reduce the crystallization temperature of alumina.
A low-temperature crystallized alumina fiber with a simple preparation method and a short production cycle has been realized. The fiber diameter is small and the surface is smooth, and the alumina can crystallize at a lower temperature.
Smart Images

Figure CN118756375A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of alumina fibers, and specifically relates to a low-temperature crystallized alumina fiber and a preparation method thereof. Background Art
[0002] Alumina fiber is a high-performance inorganic fiber with the advantages of good thermal stability, high chemical stability, low thermal conductivity and low dielectric constant. It is used in thermal insulation, high-temperature equipment and special equipment. It is used in the high-temperature flexible thermal protection system of hypersonic inflatable pneumatic reducer. The outer fabric of the system is high-temperature resistant alumina fiber. In addition, alumina fiber is also widely used in rockets, hypersonic missiles and aircraft, etc., which require thermal protection materials with strength and chemical corrosion resistance.
[0003] The main methods for preparing alumina fibers include melting method, sol-gel method, impregnation method and electrostatic spinning method. For example, the patented technology of "an alumina fiber and its preparation method" (CN 111074357B) produces high-quality fibers by controlling the mixing process of aluminum source, silicon source, other oxide sources and the first spinning aid, and the addition form and amount of the second spinning aid. However, the spinning solution of this technology needs to be aged, the overall preparation time is too long, and the fiber preparation method is complicated.
[0004] The patented technology of "a porous alumina fiber and its preparation method" (CN 117026424A) uses water-based alumina spinning nanoemulsion as raw material to prepare porous alumina fibers. Although the electrostatic spinning of this technology effectively avoids the problem of organic solvent pollution, the fiber diameter is above 1μm, which is relatively large.
[0005] José Hafid Roque-Ruiz et al. (Roque-Ruiz JH, Medellín-Castillo NA, Reyes-López S Y. Fabrication of α-alumina fibers by sol-gel and electrospinning of aluminum nitrate precursor solutions[J]. Results in Physics, 2019, 12: 193-204) used a precursor solution to prepare primary alumina fibers by electrospinning, and then obtained alumina fibers by heat treatment; however, during the heat treatment process of this technology, the alumina fibers would sinter, causing the grains to grow to form alumina particles, destroying the fiber surface morphology and making it impossible to maintain a smooth surface.
[0006] The patented technology of "A method for preparing alumina nanofibers by electrospinning" (CN 113151933A) uses electrospinning of aluminum salt and organic polymer precursor solution to prepare alumina nanofibers, but the obtained fibers need to be calcined at 1400°C. The heat treatment temperature is too high and it is difficult for alumina to crystallize at low temperatures.
[0007] At present, alumina fibers prepared by electrospinning generally have technical defects such as complex preparation method, long production cycle, large fiber diameter, rough fiber surface and difficulty in crystallizing alumina at lower temperatures. Summary of the invention
[0008] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing low-temperature crystallized alumina fibers with a simple preparation method and a short production cycle. The low-temperature crystallized alumina fibers prepared by this method have a small fiber diameter, a smooth fiber surface, and the alumina in the fibers can crystallize at a lower temperature.
[0009] To achieve the above purpose, the specific steps of the technical solution adopted by the present invention are:
[0010] Step 1, according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:1-5:0.1-1:5-20, add the spinning aid, the aluminum salt and the additive into the alcohol solution, stir until completely dissolved, and obtain the spinning solution.
[0011] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0012] The spinning solution injection flow rate is 0.01-0.2 mL / min, the distance between the spinning needle and the receiving roller is 5-20 cm, the receiving roller speed is 50-140 r / min, the spinning voltage is 5-20 kV, the spinning environment temperature is 20-40° C., and the spinning environment relative humidity is 30-60%.
[0013] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 800-1400° C. in an inert atmosphere for 1-3 hours to obtain low-temperature crystallized alumina fiber.
[0014] The spinning aid is one or more of polyvinyl butyral, polyvinyl alcohol and polyvinyl pyrrolidone; the relative molecular mass of the polyvinyl butyral is 90,000-120,000, the relative molecular mass of the polyvinyl alcohol is 85,000-100,000 and the average molecular mass of the polyvinyl pyrrolidone is 1,300,000.
[0015] The aluminum salt is one or more of aluminum acetylacetonate, aluminum chloride, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate; the aluminum salt has a purity of analytical grade or above.
[0016] The additives are graphene, graphene oxide and MXene-single-layer Ti 3 C 2 T x The purity of the graphene and graphene oxide is above 90%.
[0017] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1-1.5, mix them, and then obtain the alcohol solution.
[0018] The pre-oxidation conditions are: keeping the temperature at 100-300° C. for 1-6 hours.
[0019] The inert atmosphere is argon or nitrogen.
[0020] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0021] 1. The present invention directly adds a spinning aid, aluminum salt and additives to an alcohol solution and stirs until completely dissolved to obtain a spinning solution; the addition of a spinning aid can increase the viscosity of the spinning solution and the spinnability of the solution to form fibers with uniform properties. The present invention transfers the spinning solution to a syringe and performs electrostatic spinning under certain environments and conditions to obtain precursor fibers: the precursor fibers are first pre-oxidized and heat-treated to obtain low-temperature crystalline alumina fibers, that is, alumina fibers can be obtained through simple electrostatic spinning and heat treatment processes, and the preparation method is simple and the production cycle is short.
[0022] 2. The present invention adopts an electrostatic spinning method and configures a precursor spinning solution system, which can ensure that during the electrostatic spinning process, the spinning solution is stretched under the action of the electric field force, and the solvent is continuously volatilized to form precursor fibers. At the same time, the spinning environment and conditions are controlled to ensure that most of the solvent of the precursor fiber is evaporated when it falls on the receiving roller, the fiber remains dry, and no adhesion occurs between the fibers. In this way, the surface morphology of the precursor fiber is not destroyed during the heat treatment process, and the prepared low-temperature crystallized alumina fiber has a small diameter and a smooth surface.
[0023] 3. The present invention reduces the energy required for the oxygen ion arrangement to change from face-centered cubic to hexagonal close-packed when the transition phase of aluminum oxide changes to the high-temperature stable α phase by introducing additives while controlling the spinning solution ratio. This type of transformation belongs to the lattice reconstruction phase transition, which involves the movement of oxygen ions with a larger radius, requires more energy, and has a high crystallization temperature. It can effectively reduce the crystallization temperature of aluminum oxide in the fiber.
[0024] Therefore, the present invention has the characteristics of simple preparation method and short production cycle. The prepared low-temperature crystallized alumina fiber has a small diameter and a smooth surface, and the alumina in the fiber can be crystallized at a relatively low temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image of a low-temperature crystallized alumina fiber prepared in the present invention;
[0026] Figure 2 for Figure 1 XRD pattern of the prepared low-temperature crystallized alumina fibers. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with the accompanying drawings and specific implementation methods, but is not intended to limit the scope of protection thereof.
[0028] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0029] Step 1, according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:1-5:0.1-1:5-20, add the spinning aid, the aluminum salt and the additive into the alcohol solution, stir until completely dissolved, and obtain the spinning solution.
[0030] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0031] The spinning solution injection flow rate is 0.01-0.2 mL / min, the distance between the spinning needle and the receiving roller is 5-20 cm, the receiving roller speed is 50-140 r / min, the spinning voltage is 5-20 kV, the spinning environment temperature is 20-40° C., and the spinning environment relative humidity is 30-60%.
[0032] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 800-1400° C. in an inert atmosphere for 1-3 hours to obtain low-temperature crystallized alumina fiber.
[0033] The spinning aid is one or more of polyvinyl butyral, polyvinyl alcohol and polyvinyl pyrrolidone.
[0034] The aluminum salt is one or more of aluminum acetylacetonate, aluminum chloride, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate; the aluminum salt has a purity of analytical grade or above.
[0035] The additives are graphene, graphene oxide and MXene-single-layer Ti 3 C 2 T xThe purity of the graphene and graphene oxide is above 90%.
[0036] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1-1.5, mix them, and then obtain the alcohol solution.
[0037] The pre-oxidation conditions are: keeping the temperature at 100-300° C. for 1-6 hours.
[0038] The inert atmosphere is argon or nitrogen.
[0039] In this specific implementation:
[0040] The relative molecular mass of the polyvinyl butyral is 90,000 to 120,000, the relative molecular mass of the polyvinyl alcohol is 85,000 to 100,000, and the average molecular mass of the polyvinyl pyrrolidone is 1,300,000;
[0041] The aluminum salt is analytically pure or above;
[0042] The purity of the graphene and graphene oxide is above 90%;
[0043] The anhydrous ethanol is of analytical grade or above.
[0044] This will not be described in detail in the embodiments.
[0045] Example 1
[0046] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0047] Step 1: prepare the spinning aid: aluminum salt: additive: alcohol solution in a mass ratio of 1:1:0.1:5, add the spinning aid, the aluminum salt and the additive into the alcohol solution, and stir until they are completely dissolved to obtain a spinning solution.
[0048] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0049] The spinning solution injection flow rate is 0.01 mL / min, the distance between the spinning needle and the receiving roller is 5 cm, the receiving roller speed is 50 r / min, the spinning voltage is 5 kV, the spinning environment temperature is 20° C., and the spinning environment relative humidity is 30%.
[0050] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 800° C. under an inert atmosphere for 1 hour to obtain low-temperature crystallized alumina fiber.
[0051] In this embodiment:
[0052] The spinning aid is polyvinyl butyral.
[0053] The aluminum salt is aluminum acetylacetonate.
[0054] The additive is graphene.
[0055] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1, mix them, and then obtain the alcohol solution.
[0056] The pre-oxidation condition is: keeping warm at 100° C. for 1 hour.
[0057] The inert atmosphere is argon.
[0058] Example 2
[0059] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0060] Step 1: according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:1.3:0.2:8, the spinning aid, the aluminum salt and the additive are added into the alcohol solution, and stirred until they are completely dissolved to obtain a spinning solution.
[0061] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0062] The spinning solution injection flow rate is 0.03 mL / min, the distance between the spinning needle and the receiving roller is 8 cm, the receiving roller speed is 80 r / min, the spinning voltage is 8 kV, the spinning environment temperature is 22° C., and the spinning environment relative humidity is 35%.
[0063] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 900° C. in an inert atmosphere for 2 hours to obtain low-temperature crystallized alumina fiber.
[0064] In this embodiment:
[0065] The spinning aid is polyvinyl pyrrolidone.
[0066] The aluminum salt is aluminum chloride.
[0067] The additive is graphene oxide.
[0068] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.1, mix them, and then obtain the alcohol solution.
[0069] The pre-oxidation condition is: keeping warm at 150° C. for 2 hours.
[0070] The inert atmosphere is nitrogen.
[0071] Example 3
[0072] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0073] Step 1: according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:1.5:0.3:10, add the spinning aid, the aluminum salt and the additive into the alcohol solution, and stir until they are completely dissolved to obtain a spinning solution.
[0074] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0075] The spinning solution injection flow rate is 0.05 mL / min, the distance between the spinning needle and the receiving roller is 10 cm, the receiving roller speed is 100 r / min, the spinning voltage is 10 kV, the spinning environment temperature is 25° C., and the spinning environment relative humidity is 40%.
[0076] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 1000° C. in an inert atmosphere for 3 hours to obtain low-temperature crystalline alumina fiber.
[0077] In this embodiment:
[0078] The spinning aid is polyvinyl alcohol.
[0079] The aluminum salt is aluminum sulfate 18-hydrate.
[0080] The additive is MXene-single-layer Ti 3 C 2 T x .
[0081] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.2, mix them, and then obtain the alcohol solution.
[0082] The pre-oxidation conditions are: keeping warm at 200° C. for 3 hours.
[0083] The inert atmosphere is argon.
[0084] Example 4
[0085] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0086] Step 1: according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:2:0.4:11, the spinning aid, the aluminum salt and the additive are added to the alcohol solution, and stirred until they are completely dissolved to obtain a spinning solution.
[0087] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0088] The spinning solution injection flow rate is 0.06 mL / min, the distance between the spinning needle and the receiving roller is 12 cm, the receiving roller speed is 110 r / min, the spinning voltage is 12 kV, the spinning environment temperature is 28° C., and the spinning environment relative humidity is 45%.
[0089] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 1100° C. in an inert atmosphere for 2 hours to obtain low-temperature crystallized alumina fiber.
[0090] In this embodiment:
[0091] The spinning aid is a mixture of polyvinyl butyral and polyvinyl pyrrolidone.
[0092] The aluminum salt is aluminum nitrate nonahydrate.
[0093] The additive is a mixture of graphene and graphene oxide.
[0094] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.3, mix them, and then obtain the alcohol solution.
[0095] The pre-oxidation conditions are: keeping warm at 230° C. for 4 hours.
[0096] The inert atmosphere is nitrogen.
[0097] Example 5
[0098] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0099] Step 1: according to the mass ratio of spinning aid: aluminum salt: additive: alcohol solution of 1:2.5:0.6:12, the spinning aid, the aluminum salt and the additive are added to the alcohol solution, and stirred until they are completely dissolved to obtain a spinning solution.
[0100] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0101] The spinning solution injection flow rate is 0.1 mL / min, the distance between the spinning needle and the receiving roller is 15 cm, the receiving roller speed is 120 r / min, the spinning voltage is 16 kV, the spinning environment temperature is 30° C., and the relative humidity of the spinning environment is 50%.
[0102] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 1200° C. under an inert atmosphere for 3 hours to obtain low-temperature crystallized alumina fiber.
[0103] In this embodiment:
[0104] The spinning aid is a mixture of polyvinyl butyral and polyvinyl alcohol.
[0105] The aluminum salt is a mixture of aluminum acetylacetonate and aluminum chloride.
[0106] The additives are graphene and MXene-single-layer Ti 3 C 2 T x mixture.
[0107] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.4, mix them, and then obtain the alcohol solution.
[0108] The pre-oxidation condition is: keeping the temperature at 250° C. for 5 hours.
[0109] The inert atmosphere is argon.
[0110] Example 6
[0111] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0112] Step 1: prepare the spinning aid, aluminum salt, additive and alcohol solution in a mass ratio of 1:3:0.8:15, add the spinning aid, aluminum salt and additive into the alcohol solution, and stir until they are completely dissolved to obtain a spinning solution.
[0113] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0114] The spinning solution injection flow rate is 0.15 mL / min, the distance between the spinning needle and the receiving roller is 18 cm, the receiving roller speed is 130 r / min, the spinning voltage is 18 kV, the spinning environment temperature is 35° C., and the spinning environment relative humidity is 55%.
[0115] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 1300° C. under an inert atmosphere for 1 hour to obtain low-temperature crystallized alumina fiber.
[0116] In this embodiment:
[0117] The spinning aid is a mixture of polyvinyl pyrrolidone and polyvinyl alcohol.
[0118] The aluminum salt is a mixture of aluminum acetylacetonate and aluminum sulfate 18-hydrate.
[0119] The additives are graphene oxide and MXene-single-layer Ti 3 C 2 T x mixture.
[0120] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.3, mix them, and then obtain the alcohol solution.
[0121] The pre-oxidation conditions are: keeping warm at 280° C. for 3 hours.
[0122] The inert atmosphere is nitrogen.
[0123] Example 7
[0124] A low temperature crystallized alumina fiber and a preparation method thereof. The steps of the preparation method described in this specific embodiment are:
[0125] Step 1: prepare the spinning aid: aluminum salt: additive: alcohol solution in a mass ratio of 1:5:1:20, add the spinning aid, the aluminum salt and the additive into the alcohol solution, and stir until they are completely dissolved to obtain a spinning solution.
[0126] Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers:
[0127] The spinning solution injection flow rate is 0.2 mL / min, the distance between the spinning needle and the receiving roller is 20 cm, the receiving roller speed is 140 r / min, the spinning voltage is 20 kV, the spinning environment temperature is 40° C., and the spinning environment relative humidity is 60%.
[0128] Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 1400° C. under an inert atmosphere for 3 hours to obtain low-temperature crystallized alumina fiber.
[0129] In this embodiment:
[0130] The spinning aid is a mixture of polyvinyl butyral, polyvinyl pyrrolidone and polyvinyl alcohol.
[0131] The aluminum salt is a mixture of aluminum acetylacetonate and aluminum nitrate nonahydrate.
[0132] The additives are graphene, graphene oxide and MXene-single-layer Ti 3 C 2 T x mixture.
[0133] The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1.5, mix them, and then obtain the alcohol solution.
[0134] The pre-oxidation conditions are: keeping warm at 300° C. for 6 hours.
[0135] The inert atmosphere is argon.
[0136] Example 8
[0137] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 1:
[0138] The aluminum salt is a mixture of aluminum chloride and aluminum nitrate nonahydrate.
[0139] Example 9
[0140] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 2:
[0141] The aluminum salt is a mixture of aluminum chloride and aluminum sulfate 18-hydrate.
[0142] Example 10
[0143] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 3:
[0144] The aluminum salt is a mixture of aluminum nitrate nonahydrate and aluminum sulfate 18hydrate.
[0145] Embodiment 11
[0146] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 4:
[0147] The aluminum salt is a mixture of aluminum acetylacetonate, aluminum chloride and aluminum nitrate nonahydrate.
[0148] Example 12
[0149] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 5:
[0150] The aluminum salt is a mixture of aluminum acetylacetonate, aluminum chloride and aluminum sulfate 18-hydrate.
[0151] Embodiment 13
[0152] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 6:
[0153] The aluminum salt is a mixture of aluminum acetylacetonate, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate.
[0154] Embodiment 14
[0155] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 7:
[0156] The aluminum salt is a mixture of aluminum chloride, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate.
[0157] Embodiment 15
[0158] A low temperature crystallized alumina fiber and a preparation method thereof. Except for the aluminum salt, the rest of this embodiment is the same as that of embodiment 2:
[0159] The aluminum salt is a mixture of aluminum acetylacetonate, aluminum chloride, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate.
[0160] Compared with the prior art, this specific implementation has the following positive effects:
[0161] 1. The present invention directly adds a spinning aid, aluminum salt and additives to an alcohol solution and stirs until completely dissolved to obtain a spinning solution; the addition of a spinning aid can increase the viscosity of the spinning solution and the spinnability of the solution to form fibers with uniform properties. The present invention transfers the spinning solution to a syringe and performs electrostatic spinning under certain environments and conditions to obtain precursor fibers: the precursor fibers are first pre-oxidized and heat-treated to obtain low-temperature crystalline alumina fibers, that is, alumina fibers can be obtained through simple electrostatic spinning and heat treatment processes, and the preparation method is simple and the production cycle is short.
[0162] 2. This specific embodiment adopts the electrostatic spinning method, and the configured precursor spinning solution system can ensure that during the electrostatic spinning process, the spinning solution is stretched under the action of the electric field force, and the solvent is continuously volatilized to form the precursor fiber. At the same time, the spinning environment and conditions are controlled to ensure that most of the solvent of the precursor fiber is evaporated when it falls on the receiving roller, the fiber remains dry, and there is no adhesion between the fibers, which can ensure that the surface morphology of the precursor fiber is not destroyed during the heat treatment process. The prepared low-temperature crystallized alumina fiber is shown in the attached figure: Figure 1 This is a SEM image of the low-temperature crystallized alumina fiber prepared in Example 3; Figure 2 for Figure 1 XRD pattern of low temperature crystallized alumina fiber prepared. Figure 1It can be seen that the prepared low-temperature crystallized alumina fiber has a small diameter and a smooth surface.
[0163] 3. This specific implementation method reduces the energy required for the oxygen ion arrangement to change from face-centered cubic hexagonal close-packed when alumina changes from a transition phase to a high-temperature stable α phase by introducing additives while keeping the spinning solution ratio unchanged. This type of transformation belongs to a lattice reconstruction phase transition, which involves the movement of oxygen ions with a larger radius, requires more energy, and has a high crystallization temperature. This specific implementation method reduces the crystallization temperature of alumina by adding additives while keeping the spinning parameters the same. Figure 2 As shown, from Figure 2 It can be seen that when the alumina fiber is heat treated at 800°C, there is an obvious alumina diffraction peak in the XRD diffraction pattern of the fiber with 0.5% additive added, indicating that the addition of the additive effectively reduces the crystallization temperature of alumina.
[0164] Therefore, this specific embodiment has the characteristics of simple preparation method and short production cycle. The prepared low-temperature crystallized alumina fiber has a small diameter and a smooth surface, and the alumina in the fiber can crystallize at a relatively low temperature.
Claims
1. A method for preparing low temperature crystallized alumina fiber, characterized in that The steps of the preparation method are: Step 1, preparing the spinning aid: aluminum salt: additive: alcohol solution in a mass ratio of 1:1-5:0.1-1:5-20, adding the spinning aid, the aluminum salt and the additive into the alcohol solution, and stirring until they are completely dissolved to obtain a spinning solution; Step 2: Transfer the spinning solution to a syringe and perform electrospinning under the following environment and conditions to obtain precursor fibers: The spinning solution injection flow rate is 0.01-0.2 mL / min, the distance between the spinning needle and the receiving roller is 5-20 cm, the receiving roller speed is 50-140 r / min, the spinning voltage is 5-20 kV, the spinning environment temperature is 20-40 ° C, and the relative humidity of the spinning environment is 30-60%; Step 3: pre-oxidize the precursor fiber in a muffle furnace, and then keep it at 800-1400° C. in an inert atmosphere for 1-3 hours to obtain low-temperature crystallized alumina fiber.
2. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The spinning aid is one or more of polyvinyl butyral, polyvinyl alcohol and polyvinyl pyrrolidone; the relative molecular mass of the polyvinyl butyral is 90,000-120,000, the relative molecular mass of the polyvinyl alcohol is 85,000-100,000 and the average molecular mass of the polyvinyl pyrrolidone is 1,300,000.
3. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The aluminum salt is one or more of aluminum acetylacetonate, aluminum chloride, aluminum nitrate nonahydrate and aluminum sulfate 18hydrate; the aluminum salt has a purity of analytical grade or above.
4. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The additives are graphene, graphene oxide and MXene-single-layer Ti3C2T x The purity of the graphene and graphene oxide is above 90%.
5. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The preparation method of the alcohol solution is: prepare the ingredients according to the mass ratio of deionized water to anhydrous ethanol of 1:1-1.5, mix them, and then obtain the alcohol solution.
6. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The pre-oxidation conditions are: keeping the temperature at 100-300° C. for 1-6 hours.
7. The method for preparing low temperature crystallized alumina fiber according to claim 1, characterized in that The inert atmosphere is argon or nitrogen.
8. A low temperature crystallized alumina fiber, characterized in that The low-temperature crystallized alumina fiber is a low-temperature crystallized alumina fiber prepared by the method for preparing the low-temperature crystallized alumina fiber according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing aluminum oxide nanofiber by electrostatic spinning
CN101982581A
Method for preparing electrode material for all-vanadium flow battery
CN102522568A
Anode material of dye-sensitized solar cell doped with graphene, and manufacturing method and applications of anode material
CN103151173A
Preparation method for polycrystalline alumina fiber
CN103726131A
Preparation method of graphene oxide modified titanium dioxide nanofibers
CN106757522A