A method for preparing cotton-feel composite yarn

By combining stretching and overfeeding processes, and using a special nozzle to expand the allowance of long yarns, the long yarns are wound in an arc around the periphery of short yarns. This solves the problem of the stiff hand feel of cotton-feel composite yarns, achieving a good wool-like feel and a skin-friendly and comfortable effect, while reducing production costs.

CN118756390BActive Publication Date: 2026-11-17FUJIAN LEISHI NEW MATERIAL TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410659270.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2026-11-17
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

Existing cotton-feel composite yarns lack support, resulting in a stiff hand feel, poor wool-like and skin-friendly texture, high cost, and low production capacity.

Method used

The process combines stretching and overfeeding. A special nozzle keeps the long yarn in a relaxed state and the short yarn in a tense state. The nozzle's annular recess expands the excess length of the long yarn, causing it to wrap around the short yarn in a large arc shape, creating a three-dimensional terry effect.

Benefits of technology

The prepared cotton-feel composite yarn has a three-dimensional feel, is skin-friendly and comfortable, reduces costs, and can be produced on conventional texturing machines, resulting in a significant cost reduction compared to air-transformer machines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756390B_ABST
    Figure CN118756390B_ABST
Patent Text Reader

Abstract

This invention relates to the field of spinning technology, specifically to a method for preparing a cotton-feel composite yarn. The method includes the following steps: long yarn and short yarn are respectively fed into a nozzle through different yarn paths for winding. During winding, the long yarn is in a relaxed state, while the short yarn is in a tense state. An annular recess exists on the outer periphery of the nozzle's air jet orifice, and the distance from the axis of the annular recess to its outer diameter is ≥5mm. This method combines stretching and overfeeding, while simultaneously changing the diameter of the recessed orifice around the nozzle to extend the overfeed of the long yarn, allowing the short yarn to provide support, and the long yarn to wind around the short yarn in a large arc shape. The resulting cotton-feel composite fiber achieves a cotton-like effect in terms of feel and texture, similar to that produced by an air-changing machine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of spinning technology, specifically to a method for preparing cotton-feel composite yarn. Background Technology

[0002] In an increasingly homogenized market, the value of differentiated new fibers is becoming increasingly apparent. Traditional textured composite cotton-feel yarns utilize ultra-fine denier filaments with a diameter of less than 0.5D to create a cotton-feel effect. For example, Chinese invention patent application number 201310191029.8 discloses a method for producing cationic composite cotton-like yarn. This method uses a one-step spinning device for POY / FDY composite fibers to produce POY / FDY composite fibers, which are then false-twisted to produce composite cotton-like yarn. However, this yarn lacks a supporting skeleton, resulting in a stiffer feel. Furthermore, the two fibers in the yarn are stretched uniformly and are of equal length, resulting in a yarn without the fluffiness and tactile feel of a looped tuft, and with poor softness and skin-friendly texture. Its effect is significantly different from that of ATY (air-textured yarn), a cotton-like fiber produced by an air-textured machine. While ATY has a better feel, its production cost is high and its production capacity is low. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide a cotton-feel composite yarn with good wool feel that does not use ATY in production and its preparation method.

[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows: a method for preparing cotton-feel composite yarn, comprising the following steps: long yarn and short yarn are respectively wound into a nozzle through different yarn paths, the long yarn is in a relaxed state and the short yarn is in a tense state during winding; there is an annular depression on the outer periphery of the air jet hole of the nozzle, and the axis of the annular depression is ≥5mm to the outer diameter.

[0005] The beneficial effects of this invention are as follows: The preparation method of this invention combines stretching and overfeeding, while simultaneously changing the concave orifice diameter around the nozzle to expand the overfeed margin for the long yarn, allowing the short yarn to play a supporting role, and the long yarn to be wound around the outer periphery of the short yarn in a large arc shape. The resulting cotton-feel composite fiber can achieve the cotton-like effect produced by an air-changing machine in terms of feel and style. Attached Figure Description

[0006] Figure 1 The diagram shown is a silk path diagram of Embodiment 1 of the present invention;

[0007] Figure 2 The diagram shown is a schematic representation of the nozzle structure according to Embodiment 1 of the present invention;

[0008] Figure 3 The diagram shown is a comparative example of the present invention.

[0009] Figure 4 The image shown is a physical picture of the cotton-feel composite yarn of Embodiment 1 of the present invention;

[0010] Figure 5 The image shown is a physical picture of the composite yarn of Comparative Example 1 of the present invention.

[0011] Label Explanation:

[0012] 1. First roller; 2. Heating box; 3. Cooling plate; 4. False twister; 5. Second roller; 6. Nozzle; 61. Air jet; 62. Annular recess; 7. Zero roller; 8. Guide roller; 9. Auxiliary roller. Detailed Implementation

[0013] To explain in detail the technical content, objectives, and effects of the present invention, the following description is provided in conjunction with the embodiments and accompanying drawings.

[0014] Please refer to Figure 1 A method for preparing a cotton-feel composite yarn includes the following steps: long yarn and short yarn are wound into a nozzle through different yarn paths, the long yarn is in a relaxed state and the short yarn is in a tense state during winding; there is an annular depression on the outer periphery of the air jet hole of the nozzle, and the distance from the axis of the annular depression to the outer diameter is ≥5mm.

[0015] As described above, the beneficial effects of this invention are as follows: To improve the skin-friendly and soft effect of traditional imitation cotton and enhance the differentiated value of the product, this invention adjusts the spinning process, yarn path, and equipment. This invention utilizes a combination of stretching and overfeeding, allowing the long yarn to enter a specially designed nozzle in a relaxed state and the short yarn in a tense state. The contact points between the long and short yarns are formed by winding. At this time, the short yarn is in a tense state, preventing compressed air from bending or deforming it, thus providing support similar to the core yarn of air-textured fiber. The annular recess of the specially designed nozzle is wider than that of a conventional nozzle, altering the range of compressed air action and extending the overfeed margin for the long yarn, causing the long yarn to wind around the short yarn in a larger arc shape, resulting in greater fluffiness. The resulting cotton-feel composite fiber has a more three-dimensional feel, with loops of varying lengths, producing a fuzzy effect similar to short fiber fibers. The cotton-feel composite fiber of this invention achieves the imitation cotton effect produced by an air-textured machine in terms of feel and style.

[0016] The cotton-feel composite yarn prepared using the method of this invention has distinct curved loops, which is significantly different from composite cotton-like fibers prepared by traditional texturing machines. These loops enhance the comfort and skin-friendly feel of the fabric. Furthermore, this invention can be achieved using a texturing machine, resulting in a substantial cost reduction compared to air-conditioning machines.

[0017] Furthermore, the long yarn is POY (pre-oriented yarn), and the short yarn is DTY (draw textured yarn).

[0018] As can be seen from the above description, the present invention can achieve the cotton-like effect using POY and DTY, and the raw material cost is significantly reduced compared with the DTY of the air converter.

[0019] Furthermore, the cross-section of the long yarn is a cross section.

[0020] As can be seen from the above description, long yarns with a cross-section have a moisture-wicking effect.

[0021] Furthermore, the cotton-feel composite yarn has a density of 80–160D.

[0022] Furthermore, the long yarn is fed in by a first roller, passes through a heating box, a cooling plate, a false twister and a second roller in sequence, and is wound with the short yarn fed in by a zero roller at the nozzle. The resulting composite yarn is then fed into a package via an auxiliary roller.

[0023] As described above, the heat-set yarn bundles shrink and harden, making them difficult to disperse when passing through the nozzle. Furthermore, the nozzle used in this invention has a wider annular recess, resulting in less compressed air impact force, making it difficult to perform composite winding on the heat-set yarn bundles. Therefore, the long yarns of this invention do not undergo heat setting after false twisting before entering the nozzle.

[0024] Furthermore, the D / Y ratio of the long yarn is 0.85 to 1.0 when it passes through the false twister.

[0025] As described above, the D / Y ratio of the long yarn is 0.85–1.0 when it passes through the false twister. , The yarn has a high crimp, making it more suitable for forming curves.

[0026] Furthermore, the temperature of the hot box is 150–195°C.

[0027] Furthermore, the speed ratio between the zero roller and the auxiliary roller is 1:1.3 to 1.4.

[0028] As can be seen from the above description, the speed ratio of the zero roller and the auxiliary roller is 1:1.3 to 1.4, which keeps the short yarn under tension.

[0029] Furthermore, the speed ratio between the first roller and the second roller is 1:1.7 to 1.8.

[0030] Furthermore, the speed ratio between the second roller and the auxiliary roller is 1:0.8 to 0.9.

[0031] As can be seen from the above description, the long yarn enters the nozzle using an overfeed process and wraps around the short yarn under tension, which can produce loops of different sizes.

[0032] Furthermore, the depth of the annular depression gradually decreases from the distance from the axis to the outer diameter.

[0033] As can be seen from the above description, the depth of the annular depression gradually decreases from the distance from the axis to the outer diameter, and the overfed long yarn can expand the allowance of the long yarn under the action of compressed air with a relatively low flow rate.

[0034] Please refer to Figure 1 and 2 Embodiment 1 of the present invention is: a method for preparing a cotton-feel composite yarn, comprising the following steps:

[0035] S1: Using a Barmag EFK-1000 texturing machine, the long yarn is fed in by the first roller 1, and passes through the heating box 2, cooling plate 3, false twister 4 and second roller 5 in sequence, and enters the nozzle 6;

[0036] S2: Short yarn is fed in by zero roller 7, passes through guide 8 and enters nozzle 6;

[0037] S3: A guide hook is provided below the nozzle 6 to allow long yarns and short yarns to be arranged side by side. The long yarns in a relaxed state and the short yarns in a tense state are wound together under the action of the nozzle. The nozzle is 25mm long and 9mm thick. The diameter of the air jet hole is 1mm. There is an annular recess 62 on the outer periphery of the air jet hole 61 of the nozzle. The depth of the annular recess 62 gradually decreases from the axis to the outer diameter. The distance from the axis to the outer diameter of the annular recess 62 is 5mm.

[0038] S4: The composite yarn after winding is 100D and enters the package via auxiliary roller 9.

[0039] The specifications of the long yarn and short yarn in Example 1 are shown in Table 1, and the specific process parameters are shown in Table 2.

[0040] Table 1

[0041]

[0042] Table 2

[0043]

[0044] Embodiment 2 of the present invention is as follows:

[0045] The only difference between Example 2 and Example 1 is that: the distance from the axis of the annular recess of the nozzle to the outer diameter is 6mm; the speed ratio of the zero roller and the auxiliary roller is 1:1.3, the speed ratio of the first roller and the second roller is 1:1.7, and the speed ratio of the second roller and the auxiliary roller is 1:0.8; the false twist D / Y ratio is 0.85; and the cotton-feel composite yarn is 80D.

[0046] Embodiment 2 of the present invention is as follows:

[0047] The only difference between Example 2 and Example 1 is that the speed ratio of zero roller to auxiliary roller is 1:1.4, the speed ratio of one roller to two rollers is 1:1.8, and the speed ratio of two rollers to auxiliary rollers is 1:0.9; the false twist D / Y ratio is 1.0; and the cotton-feel composite yarn is 160D.

[0048] Comparative Example 1 of the present invention is:

[0049] The only difference between Comparative Example 1 and Example 1 is that both long and short yarns are fed in by a roller 1, passing sequentially through a heating box 2, a cooling plate 3, a false twister 4, and a second roller 5, before entering the nozzle 6 for winding. The wound composite yarn then enters the packaged yarn path via an auxiliary roller 9. Figure 3 .

[0050] The composite yarns prepared in Example 1 and Comparative Example 1 are shown in the figures below. Figure 4 and Figure 5 The properties of the two composite yarns were tested, and the test results are shown in Table 3.

[0051] Table 3

[0052]

[0053] Depend on Figure 4 and Figure 5 As can be seen, the composite yarn prepared by this invention has long yarns wrapped around the periphery of short yarns in a larger arc shape, making it more fluffy. Table 3 shows that the long-short AB type composite cotton-feel yarn prepared by this invention has only a slight decrease in strength and elongation compared to traditional parallel AB composite cotton-feel yarn, meeting the requirements for fibers.

[0054] In summary, the method for preparing cotton-feel composite yarn provided by this invention has the following advantages:

[0055] 1. By combining stretching and overfeeding, and simultaneously changing the size of the recess around the nozzle, the overfeed allowance for the long yarn is expanded, causing the long yarn to wrap around the outer periphery of the supporting short yarn in a larger arc shape. This produces a cotton-like composite fiber with a more three-dimensional feel and a looped effect of varying lengths.

[0056] 2. The cotton-like effect can be achieved by using POY and DTY and conventional texturing machines. Compared with DTY from air-transformer, the cost of raw materials and equipment is significantly reduced.

[0057] 3. The cross-section of the long yarn used is a cross section, which gives the resulting cotton-feel composite yarn good moisture absorption and perspiration wicking effect.

[0058] 4. The prepared cotton-feel composite yarn shrinks during subsequent weaving and heat setting processes, resulting in a velvety appearance on the surface of the woven fabric.

[0059] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent modifications made based on the content of the present invention specification and drawings, or direct or indirect applications in related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A method for preparing a cotton-feel composite yarn, characterized in that, Includes the following steps: A Barmag EFK-1000 texturing machine is used to wind long and short yarns into the nozzle through different yarn paths. The long yarn is fed into the nozzle using an overfeed process. During winding, the long yarn is in a relaxed state, while the short yarn is in a tense state. The long yarn is wound around the outer periphery of the short yarn in a large arc shape. There is an annular depression on the outer periphery of the air jet hole of the nozzle. The distance from the axis of the annular depression to the outer diameter is ≥5mm. The long yarn is fed in by a first roller, passes sequentially through a heating box, a cooling plate, a false twister, and a second roller, and is wound at the nozzle with a short yarn fed in by a zero roller. The resulting composite yarn is then fed into a package via an auxiliary roller. The speed ratio between the zero roller and the auxiliary roller is 1:1.3~1.4; The speed ratio of the second roller and the auxiliary roller is 1:0.8~0.9; In this process, the long yarn enters the nozzle without undergoing heat setting after false twisting.

2. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The long yarn is POY, and the short yarn is DTY.

3. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The cross-section of the long yarn is a cross section.

4. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The cotton-feel composite yarn has a density of 80~160D.

5. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The D / Y ratio of the long yarn is 0.85~1.0 when it passes through the false twister.

6. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The temperature of the hot box is 150~195℃.

7. The method for preparing cotton-feel composite yarn according to claim 1, characterized in that, The speed ratio of the first roller and the second roller is 1:1.7~1.8.

Citation Information

Patent Citations

  • Method for producing cationic type composite cotton yarn imitation threads

    CN103320923A

  • Multicomponent yarn or sewing thread texturising - uses compressed air pulses on wound core to fix cladding to core by sections

    DE2628774B1

  • Composite yarn composed of filament yarn and staple fiber and method for producing the same

    JP2005330629A

  • Opened fiber material expanding unit, jig for adjusting width and method for manufacturing opened fiber material