Anti-ultraviolet functional fabric, preparation method and anti-ultraviolet clothes
By blending polyester fiber with porous modified polyacrylonitrile fiber and adding anti-UV agents and additives, the problems of uneven UV resistance and poor washout resistance of existing fabrics are solved, achieving efficient and long-lasting UV protection and Comfortable feel.
Patent Information
- Application Number
- CN202410762928.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-11
AI Technical Summary
Existing anti-UV fabrics have poor anti-UV effect in local areas and the anti-UV agent is easy to fall off after washing, resulting in reduced UV resistance of the fabric.
It is blended with polyester fiber and porous modified polyacrylonitrile fiber. By adding anti-UV agent and additives, the porous structure is used to improve the adhesion and distribution uniformity of the anti-UV agent, and the reinforced fiber and anti-UV agent are processed by plasma equipment. interaction force.
It significantly improves the UV resistance and durability of the fabric, maintains excellent physical properties and comfortable feel, and is suitable for outdoor and sun protection needs.
Smart Images

Figure BDA0004891572880000081
Abstract
Description
Technical Field
[0001] The present application relates to the field of textile technology, and more specifically, to an anti-ultraviolet functional fabric, a preparation method and anti-ultraviolet clothing. Background Art
[0002] With the intensification of global climate change and environmental pollution, the impact of ultraviolet radiation on human health is becoming increasingly significant. Especially in outdoor activities, long-term ultraviolet radiation can not only cause skin sunburn and aging, but also increase the risk of skin cancer. Therefore, people's demand for anti-ultraviolet products is gradually increasing, especially in the textile industry, the development of efficient, comfortable and durable anti-ultraviolet fabrics has become an important trend in the development of the industry.
[0003] At present, there are some anti-UV fabric products in the textile industry. Anti-UV fabrics mainly rely on two mechanisms to achieve protection against UV rays: absorption and reflection. This is usually achieved by adding specific chemicals or finishing agents to fibers or fabrics. These substances are called anti-UV finishing agents or anti-UV agents. UV absorbers can strongly absorb UV rays and convert their energy into heat or other forms of energy, thereby reducing the damage of UV rays to the skin. Common UV absorbers include organic compounds such as benzophenone compounds and benzotriazole compounds. UV shielding agents reflect UV rays back from the surface of the fabric by reflection and scattering, thereby reducing the radiation of UV rays to the human body. Common UV shielding agents include some metal oxides, such as zinc oxide and titanium dioxide.
[0004] However, the composition, concentration and uniformity of the UV absorber in the fiber may affect the final anti-UV effect. If the concentration of the additive is insufficient or the distribution is uneven, the fabric will have poor anti-UV effect in some areas. Secondly, the bonding force between the UV absorber and the fiber will also affect the fabric's anti-UV performance. After multiple washings, the UV absorber attached to the fiber is prone to fall off, which significantly reduces the fabric's anti-UV ability. Summary of the invention
[0005] In order to improve the anti-ultraviolet effect of fabrics, the present application provides an anti-ultraviolet functional fabric, a preparation method and anti-ultraviolet clothing.
[0006] In the first aspect, the present application provides an anti-ultraviolet functional fabric adopting the following technical solution: An anti-ultraviolet functional fabric comprises a blended yarn, an anti-ultraviolet agent and an auxiliary agent. The blended yarn comprises polyester fiber and porous polyacrylonitrile fiber. The added mass of the anti-ultraviolet agent is 0.5-5% of the weight of the blended yarn, and the added amount of the auxiliary agent is 2-8% of the weight of the blended yarn.
[0007] By adopting the above technical scheme, polyester fiber has excellent durability and wrinkle resistance due to its good wear resistance, elastic recovery and wrinkle resistance. At the same time, polyester fiber also has good light resistance, which helps to maintain the color brightness and stability of the fabric. The large specific surface area of porous polyacrylonitrile fiber enables the anti-ultraviolet agent to be better dispersed and attached to the fiber. This not only improves the anti-ultraviolet performance of the fabric, but also helps the uniform distribution and durability of other functional additives. When polyester fiber and porous polyacrylonitrile fiber are blended, the advantages of the two can complement each other. Polyester fiber provides excellent physical properties and light resistance, while porous polyacrylonitrile fiber enhances the moisture absorption and perspiration performance, breathability and anti-ultraviolet performance of the fabric. In addition, the blended fabric may also have a better feel and wearing comfort.
[0008] Optionally, the preparation method of the porous polyacrylonitrile fiber is: Mix 50-60 parts of polyacrylonitrile and 60-80 parts of N,N-dimethylformamide by weight, heat and stir to make them evenly dissolved, to obtain a spinning solution; Filter the dissolved spinning solution to remove undissolved impurities, add 20-40 parts of pore-forming agent to the spinning solution, and stir it thoroughly to make it evenly dispersed; The spinning solution is extruded and spun, heated to 120-150° C., and immersed in a water tank containing deionized water for 10-30 minutes to form a polyacrylonitrile fiber matrix, and the obtained polyacrylonitrile fiber matrix is immersed in an immersion tank containing a polyvinyl amide-6 solution with a mass concentration of 10%-20% for 1-3 hours; The impregnated polyacrylonitrile fiber matrix is placed in an oxidation furnace for oxidation treatment at a temperature of 200-280° C. for about 30-60 minutes, and porous polyacrylonitrile fibers are obtained after the oxidation treatment.
[0009] Optionally, the pore-forming agent is ammonium carbonate or ammonium bicarbonate.
[0010] By adopting the above technical scheme, the obtained polyacrylonitrile fiber matrix is immersed in an impregnation tank containing a polyvinyl amide-6 solution, and after a certain period of impregnation treatment, a protective film can be formed on the fiber surface. This protective film can prevent the fiber from being over-oxidized during the subsequent oxidation treatment process, and at the same time promote the formation of more pores inside the fiber. The fiber after oxidation treatment has an excellent porous structure, and these pores can significantly improve the specific surface area and adsorption performance of the fiber. Ammonium carbonate or ammonium bicarbonate is used as a pore-forming agent, which will decompose and produce gas after heating, thereby forming a large number of voids in the polyacrylonitrile fiber, increasing the specific surface area of the fiber, which is beneficial to improving the adsorption and binding ability of the polyacrylonitrile fiber to the anti-ultraviolet agent and improving the anti-ultraviolet performance of the fabric.
[0011] Optionally, the porous polyacrylonitrile fiber needs to be modified to obtain porous modified polyacrylonitrile fiber, and the preparation method of the porous modified polyacrylonitrile fiber is: 50-60 parts by weight of porous polyacrylonitrile fiber are placed in an argon environment, the temperature is maintained at 50-80°C, the pressure is 0.1-0.5atm, 10-20 parts of butyl acrylate are mixed with the porous polyacrylonitrile fiber, and the power is 100-150W / cm 2 The plasma equipment is used to treat the butyl acrylate and the surface of the polyacrylonitrile fiber to cause graft copolymerization reaction; The grafted fiber is taken out, washed to remove the unreacted butyl acrylate, and then vacuum dried and solidified to obtain porous modified polyacrylonitrile fiber.
[0012] By adopting the above technical solution, plasma equipment is used to treat butyl acrylate and the surface of porous polyacrylonitrile fiber to undergo graft copolymerization reaction, which not only realizes the chemical bonding between butyl acrylate and the fiber surface, but also enhances the interaction between the fiber and the anti-ultraviolet agent by introducing new functional groups, thereby significantly improving the adhesion of the anti-ultraviolet agent. After modification, more active groups are introduced into the fiber surface, providing more attachment points for the anti-ultraviolet agent, which is conducive to the uniform distribution and high efficiency of the anti-ultraviolet agent.
[0013] Optionally, the anti-ultraviolet agent includes 50-70% butyl methoxydibenzoylmethane and 30-50% nano titanium dioxide.
[0014] By adopting the above technical solution, butyl methoxydibenzoylmethane can absorb long-wave dark spot effect ultraviolet rays (UVA), which can penetrate deep into the dermis of the skin and cause long-term damage to the skin. Nano-titanium dioxide can scatter and reflect ultraviolet rays, effectively protecting UVB and part of UVA. The combination of these two ingredients can provide comprehensive ultraviolet protection and effectively reduce the damage of ultraviolet rays to the skin. And continuous sunlight exposure will reduce the effectiveness of butyl methoxydibenzoylmethane in blocking UVA. However, nano-titanium dioxide has good stability and is not easily affected by light. Therefore, the combination of these two ingredients can complement each other's shortcomings and improve the durability of the sunscreen effect.
[0015] Optionally, the auxiliary agent includes polyethylene glycol and polysorbate in a mass ratio of (3-4):2.
[0016] By adopting the above technical solution, polysorbate, as a nonionic surfactant, can reduce the surface tension of the liquid, making it easier for the anti-ultraviolet agent to spread and adhere to the fiber surface. At the same time, it can form a stable complex with the anti-ultraviolet agent to further enhance its adhesion. The introduction of polyethylene glycol can increase the water retention and softness of the fiber, thereby reducing the loss of the anti-ultraviolet agent due to mechanical action during the washing process. The synergistic effect of polyethylene glycol and polysorbate in the fiber can further enhance the adhesion and wash resistance of the anti-ultraviolet agent.
[0017] In a second aspect, the present application provides a method for preparing an anti-ultraviolet functional fabric, using the following technical solution: A method for preparing an anti-ultraviolet functional fabric, comprising the following steps: The polyester fiber monofilament and the porous polyacrylonitrile fiber monofilament are mixed and spun in a ratio of 5:(2-4) to obtain a blended yarn, and the blended yarn is soaked in water and then squeezed out excess water through a roller machine; The anti-ultraviolet agent and the auxiliary agent are mixed to obtain a spraying liquid, and deionized water is added to the spraying liquid, wherein the amount of deionized water added is 60-80% of the weight of the spraying liquid; The spraying liquid is evenly sprayed on the surface of the blended yarn, and the blended yarn is sent to a vacuum drying device for drying. The blended yarn is then woven into a fabric of a desired size. The fabric is washed and dried to obtain an anti-ultraviolet functional fabric.
[0018] By adopting the above technical solution, the porous polyacrylonitrile fiber is specially modified, and the functional groups such as butyl acrylate grafted on its surface not only improve the adhesion between the fiber and the anti-ultraviolet agent, but also enhance the anti-ultraviolet performance of the fiber itself. Combined with the strength and durability of polyester fiber, the fabric made of blended yarn can provide excellent ultraviolet protection. The mixed spinning of polyester fiber and porous modified polyacrylonitrile fiber not only retains the strength and wear resistance of polyester fiber, but also increases the air permeability and moisture absorption of the fabric through the introduction of porous modified polyacrylonitrile fiber.
[0019] In a third aspect, the present application provides an anti-ultraviolet clothing, which adopts the following technical solution: The utility model relates to an anti-ultraviolet clothing made of anti-ultraviolet functional fabric.
[0020] In summary, this application has the following beneficial effects: 1. Since the present application uses polyester fiber and porous modified polyacrylonitrile fiber as blended yarn, by adding 0.5-5% by mass of anti-ultraviolet agent and 2-8% by mass of auxiliary agent, it not only inherits the wear resistance, wrinkle resistance and light resistance of polyester fiber, but also significantly enhances the moisture absorption and perspiration performance, air permeability and anti-ultraviolet performance of the fabric due to the introduction of porous modified polyacrylonitrile fiber. The blending of the two makes the fabric have excellent anti-ultraviolet effect and comfortable hand feel while maintaining excellent physical properties, and is suitable for a variety of outdoor and sun protection needs.
[0021] 2. In the present application, porous polyacrylonitrile fiber is preferably used through multiple processes such as preparation of spinning solution, spinning, addition of pore-forming agent, impregnation treatment and oxidation treatment to form a fiber matrix with excellent porous structure. Among them, ammonium carbonate or ammonium bicarbonate is used as a pore-forming agent to effectively increase the specific surface area of the fiber, thereby enhancing the adsorption and binding ability of the anti-ultraviolet agent. The porous polyacrylonitrile fiber is modified and plasma technology is used to make butyl acrylate and the fiber surface undergo graft copolymerization reaction, which not only strengthens the chemical bonding between the fiber and the anti-ultraviolet agent, but also introduces new functional groups, further improving the adhesion of the anti-ultraviolet agent and the anti-ultraviolet performance of the fabric. In summary, the present application not only optimizes the physical and chemical properties of the fiber, but also significantly enhances the anti-ultraviolet ability of the final fabric, providing a high-performance fiber material for the outdoor and sun protection fields.
[0022] 3. The method of the present application is to mix polyester fiber and porous modified polyacrylonitrile fiber to form a blended yarn, and then soak it in water, spray a spray liquid containing an anti-ultraviolet agent and an auxiliary agent, and vacuum dry it, so as to finally obtain a fabric with excellent ultraviolet protection effect. This preparation method utilizes the special modification of porous modified polyacrylonitrile fiber to enhance the adhesion between the fiber and the anti-ultraviolet agent and the anti-ultraviolet performance of the fiber itself, and at the same time combines the strength and durability of polyester fiber, so that the fabric has excellent ultraviolet protection ability and maintains good air permeability and moisture absorption. DETAILED DESCRIPTION
[0023] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0024] Preparation example of porous polyacrylonitrile fiber Preparation Example 1 The preparation method of porous polyacrylonitrile fiber is as follows: 55 kg of polyacrylonitrile and 70 kg of N,N-dimethylformamide were mixed in a reaction container, heated to 160° C. and stirred to make them evenly dissolved, to obtain a spinning solution; The dissolved spinning solution is filtered through a filter to remove undissolved impurities, the spinning solution is cooled to room temperature, 30 kg of ammonium bicarbonate is added to the spinning solution, and it is fully stirred to be evenly dispersed; The spinning solution is spun through an extrusion spinning machine and the extruded monofilament fiber is heated to 130° C. The monofilament diameter is 30 μm. After the spinning is completed, the monofilament fiber is immersed in a water tank containing deionized water for 20 minutes to form a polyacrylonitrile fiber matrix. The obtained polyacrylonitrile fiber matrix is immersed in an immersion tank containing a polyvinyl amide-6 solution with a mass concentration of 15% for 2 hours; The impregnated polyacrylonitrile fiber matrix is placed in an oxidation furnace for oxidation treatment. The oxidation treatment temperature is 250° C. and the treatment time is about 40 minutes. After completion, porous polyacrylonitrile fiber is obtained.
[0025] Preparation Example 2 The preparation method of porous polyacrylonitrile fiber is as follows: the difference from Preparation Example 1 is that 20 kg of ammonium bicarbonate is added to the spinning solution.
[0026] Preparation Example 3 The preparation method of porous polyacrylonitrile fiber is as follows: the difference from Preparation Example 1 is that 40 kg of ammonium bicarbonate is added to the spinning solution.
[0027] Preparation Example 4 The preparation method of porous polyacrylonitrile fiber is as follows: the difference from Preparation Example 1 is that 10 kg of ammonium bicarbonate is added to the spinning solution.
[0028] Preparation Example 5 The preparation method of porous polyacrylonitrile fiber is as follows: the difference from Preparation Example 1 is that 50 kg of ammonium bicarbonate is added to the spinning solution.
[0029] Preparation Example 6 The preparation method of porous polyacrylonitrile fiber is as follows: the difference from Preparation Example 1 is that 30 kg of ammonium carbonate is added to the spinning solution.
[0030] Preparation example of porous modified polyacrylonitrile fiber Preparation Example 7 The preparation method of porous modified polyacrylonitrile fiber is: 55 kg of porous polyacrylonitrile fiber obtained in Preparation Example 1 was placed in an argon environment, the temperature was maintained at 60 ° C, the pressure was 0.3 atm, 15 kg of butyl acrylate was mixed with the porous polyacrylonitrile fiber, and the power was 130 W / cm 2 The plasma machine is used for treatment to make butyl acrylate and the surface of polyacrylonitrile fiber undergo graft copolymerization reaction; The grafted fibers were taken out, washed with anhydrous ethanol and deionized water mixed in a mass ratio of 1:1 to remove unreacted butyl acrylate, and then vacuum dried and cured at 100°C to obtain porous modified polyacrylonitrile fibers.
[0031] Preparation Example 8 The preparation method of porous modified polyacrylonitrile fiber is as follows: the difference from Preparation Example 7 is that 10 kg of butyl acrylate is mixed with the porous polyacrylonitrile fiber.
[0032] Preparation Example 9 The preparation method of porous modified polyacrylonitrile fiber is as follows: the difference from Preparation Example 7 is that 20 kg of butyl acrylate is mixed with the porous polyacrylonitrile fiber. Example
[0033] Example 1 A method for preparing an anti-ultraviolet functional fabric: A polyester fiber monofilament having a diameter of 40 μm and a porous polyacrylonitrile fiber monofilament having a diameter of 30 μm were prepared.
[0034] Using a blending braiding machine, every 5 polyester fiber monofilaments and every 3 porous modified polyacrylonitrile fiber monofilaments are mixed and woven into a blended yarn with a twist of 600 TPM.
[0035] Completely immerse 10kg of woven blended yarn in clean water to allow it to fully absorb water, then pass it through a roller press to squeeze out excess water from the blended yarn through the pressure between the rollers, ensuring that the blended yarn is in a slightly wet state before spraying to facilitate the adhesion of the spray liquid.
[0036] 300 g of anti-ultraviolet agent and 500 g of auxiliary agent were added into a clean container and stirred to mix evenly, and then 560 g of deionized water was added, and magnetic stirring was performed for 5 minutes to obtain a spraying liquid.
[0037] Use a spraying device to evenly spray the spray liquid on the surface of the blended yarn, wait for the spray liquid surface to dry before spraying again, and repeat several times until the spray liquid is exhausted.
[0038] The sprayed blended yarn is sent to a vacuum drying device for drying, and the dried blended yarn is woven into a plain weave cloth with a warp yarn density of 160 threads per inch and a weft yarn density of 120 threads per inch.
[0039] The woven fabric is washed to remove impurities and residues on the surface, and the washed fabric is sent to the drying equipment again to be dried at 60°C.
[0040] The porous modified polyacrylonitrile fiber monofilament is prepared by Preparation Example 1, the anti-ultraviolet agent is 180g of butyl methoxydibenzoylmethane and 120g of nano titanium dioxide, and the auxiliary agent is 318g of polyethylene glycol and 182g of polysorbate.
[0041] Example 2 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber monofilament is prepared by Preparation Example 2.
[0042] Example 3 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber monofilament is prepared by Preparation Example 3.
[0043] Example 4 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber monofilament is prepared by Preparation Example 6.
[0044] Example 5 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber is replaced by modified polyacrylonitrile fiber, and the modified polyacrylonitrile fiber monofilament is prepared by Preparation Example 7.
[0045] Example 6 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 5 is that the modified polyacrylonitrile fiber monofilament is prepared by Preparation Example 8.
[0046] Example 7 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 5 is that the modified polyacrylonitrile fiber monofilament is prepared by Preparation Example 9.
[0047] Comparative Example Comparative Example 1 A method for preparing an anti-ultraviolet functional fabric: the difference from Example 1 is that a polyacrylonitrile fiber monofilament with a diameter of 30 μm is used.
[0048] Comparative Example 2 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber monofilament is prepared by Preparation Example 4.
[0049] Comparative Example 3 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that the porous polyacrylonitrile fiber monofilament is prepared by Preparation Example 5.
[0050] Comparative Example 4 A method for preparing an anti-ultraviolet functional fabric: the difference from Example 1 is that the anti-ultraviolet agent is 100g of butyl methoxydibenzoylmethane and 200g of nano titanium dioxide.
[0051] Comparative Example 5 A method for preparing an anti-ultraviolet functional fabric: The difference from Example 1 is that every 3 polyester fiber monofilaments and every 5 porous modified polyacrylonitrile fiber monofilaments are mixed and woven into a blended yarn.
[0052] Performance testing Detection Methods According to GB / T 18830 "Evaluation of UV Protection of Textiles", the UPF and UVA transmittance of the anti-ultraviolet fabrics prepared in Examples 1-7 and Comparative Examples 1-5 were respectively measured, and then washed for 4 hours at a water temperature of 40°C and a stirring speed of 120 r / min with the same mass of detergent of the same brand added. After washing, rinse with clean water for 30 minutes, and naturally dry at room temperature before re-measuring the UPF and UVA transmittance. The length change of the fabric after washing was recorded, and the deformation rate was calculated.
[0053] Table 1 Test data Combining Example 1 and Comparative Example 1 with Table 1, it can be seen that the porous polyacrylonitrile fiber has a large specific surface area, which allows the anti-ultraviolet agent to be better dispersed and attached to the fiber. This not only improves the anti-ultraviolet performance of the fabric, but also helps the uniform distribution and durability of other functional additives.
[0054] It can be seen from Example 1 and Comparative Examples 2-3 and Table 1 that the pore-forming agent will decompose and generate gas after heating, thereby forming a large number of voids in the polyacrylonitrile fiber, increasing the specific surface area of the fiber, which is beneficial to improving the adsorption and binding ability of the polyacrylonitrile fiber for the anti-ultraviolet agent. However, if the amount added is too much, the strength of the fiber will be seriously affected, causing the fabric to deform and be damaged during the washing process, thereby reducing the anti-ultraviolet ability of the fabric. On the contrary, if the amount added is too little, the porosity is low, the number of points that can adsorb and bind the anti-ultraviolet agent becomes less, and the effect is not good.
[0055] It can be seen from Example 1 and Comparative Example 4 and Table 1 that the effect achieved by the addition ratio of butyl methoxydibenzoylmethane and nano-titanium dioxide in the present application is better than that outside the scope of the present application.
[0056] Combining Example 1 and Comparative Example 5 with Table 1, it can be seen that the porous modified polyacrylonitrile fiber combined with the strength and durability of polyester fiber, the fabric made of blended yarn can provide excellent UV protection. The blended yarn ratio in this application takes into account both the UV resistance and the strength of the clothing fabric.
[0057] Combining Examples 1 and 4 with Table 1, it can be seen that under the same preparation conditions, the effect achieved by using ammonium bicarbonate as the pore-forming agent is better than that achieved by using ammonium carbonate.
[0058] It can be seen from Examples 1 and 5 and Table 1 that the use of plasma equipment to cause a graft copolymerization reaction between butyl acrylate and the surface of porous polyacrylonitrile fiber not only achieves chemical bonding between butyl acrylate and the fiber surface, but also enhances the interaction between the fiber and the anti-ultraviolet agent by introducing new functional groups, thereby significantly improving the adhesion of the anti-ultraviolet agent.
[0059] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A UV-resistant functional fabric, It is characterized in that The invention comprises a blended yarn, an anti-ultraviolet agent and an auxiliary agent. The blended yarn comprises polyester fiber and porous polyacrylonitrile fiber. The added amount of the anti-ultraviolet agent is 0.5-5% of the weight of the blended yarn, and the added amount of the auxiliary agent is 2-8% of the weight of the blended yarn.
2. The anti-ultraviolet functional fabric according to claim 1, Features: The preparation method of the porous polyacrylonitrile fiber is: Mix 50-60 parts of polyacrylonitrile and 60-80 parts of N,N-dimethylformamide by weight, heat and stir to make them evenly dissolved, to obtain a spinning solution; Filter the dissolved spinning solution to remove undissolved impurities, add 20-40 parts of pore-forming agent to the spinning solution, and stir it thoroughly to make it evenly dispersed; The spinning solution is extruded and spun, heated to 120-150° C., and immersed in a water tank containing deionized water for 10-30 minutes to form a polyacrylonitrile fiber matrix, and the obtained polyacrylonitrile fiber matrix is immersed in an immersion tank containing a polyvinyl amide-6 solution with a mass concentration of 10%-20% for 1-3 hours; The impregnated polyacrylonitrile fiber matrix is placed in an oxidation furnace for oxidation treatment at a temperature of 200-280° C. for about 30-60 minutes, and porous polyacrylonitrile fibers are obtained after the oxidation treatment.
3. The anti-ultraviolet functional fabric according to claim 2, Features: The pore-forming agent is ammonium carbonate or ammonium bicarbonate.
4. The anti-ultraviolet functional fabric according to claim 2, Features: The porous polyacrylonitrile fiber also needs to be modified to obtain porous modified polyacrylonitrile fiber. The preparation method of the porous modified polyacrylonitrile fiber is as follows: 50-60 parts by weight of porous polyacrylonitrile fiber are placed in an argon environment, the temperature is maintained at 50-80°C, the pressure is 0.1-0.5atm, 10-20 parts of butyl acrylate are mixed with the porous polyacrylonitrile fiber, and the power is 100-150W / cm 2 The plasma equipment is used to treat the butyl acrylate and the surface of the polyacrylonitrile fiber to cause graft copolymerization reaction; The grafted fiber is taken out, washed to remove the unreacted butyl acrylate, and then vacuum dried and solidified to obtain porous modified polyacrylonitrile fiber.
5. The anti-ultraviolet functional fabric according to claim 1, Features: The anti-ultraviolet agent comprises 50-70% of butyl methoxydibenzoylmethane and 30-50% of nano titanium dioxide.
6. The anti-ultraviolet functional fabric according to claim 1, Features: The auxiliary agent comprises polyethylene glycol and polysorbate in a mass ratio of (3-4):
2.
7. A method for preparing the anti-ultraviolet functional fabric according to any one of claims 1 to 6, Features: The following steps are involved: The polyester fiber monofilament and the porous polyacrylonitrile fiber monofilament are mixed and spun in a ratio of 5:(2-4) to obtain a blended yarn, and the blended yarn is soaked in water and then squeezed out excess water through a roller machine; The anti-ultraviolet agent and the auxiliary agent are mixed to obtain a spraying liquid, and deionized water is added to the spraying liquid, wherein the amount of deionized water added is 60-80% of the weight of the spraying liquid; The spraying liquid is evenly sprayed on the surface of the blended yarn, and the blended yarn is sent to a vacuum drying device for drying. The blended yarn is then woven into a fabric of a desired size. The fabric is washed and dried to obtain an anti-ultraviolet functional fabric. 8.Anti-ultraviolet clothing, Features: The anti-ultraviolet clothing is made from the anti-ultraviolet functional fabric described in claim 7.
Citation Information
Patent Citations
Method for dyeing, modifying and decorating surface of polypropylene material
CN101092793A
Porous polyacrylonitrile fibers and preparation method and application thereof
CN106894105A
A composite electrode material used for intelligent textiles and a preparation method thereof
CN109003837A
Full-wave-band ultraviolet sunscreen lotion and preparation method thereof
CN113332213A
Anti-ultraviolet composite fabric and preparation method thereof
CN114351324A