Sintering method of sintered neodymium-iron-boron magnet and sintered neodymium-iron-boron magnet

Through the three-stage sintering process and temperature control, the problem of rare earth precipitation on the surface of sintered NdFeB magnets is solved, the yield and performance of the magnets are improved, and the cost is reduced.

CN118762918AInactive Publication Date: 2024-10-11MIANYANG JUXING PERMANENT MAGNET MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411049553.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the sintered NdFeB magnet is cooled to room temperature and then heated to 520°C to 540°C, a large amount of rare earth precipitates on the surface, forming spots or spherical particles with high rare earth content, resulting in low product yield and affected performance.

Method used

A three-stage sintering process is adopted: sintering, high-temperature aging and low-temperature aging. The temperature is controlled between 300°C and 1100°C. The process parameters are adjusted through multiple inspections to reduce rare earth precipitation and ensure sufficient space between the magnet and the sintering box.

Benefits of technology

It effectively reduces the appearance of rare earth spots or spherical particles, improves the yield and performance of magnets, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118762918A_ABST
    Figure CN118762918A_ABST
Patent Text Reader

Abstract

The invention discloses a sintering method of a sintered neodymium-iron-boron magnet and the sintered neodymium-iron-boron magnet, and relates to the technical field of preparation of the sintered neodymium-iron-boron magnet, a magnet green body is sequentially subjected to three stages of sintering, high-temperature aging and low-temperature aging, and the sintering stage is as follows: after the magnet green body is sintered, the magnet green body is cooled to T1 along with a furnace and then subjected to heat preservation, and T1 is greater than or equal to 300 DEG C; in the high-temperature aging stage, after heat preservation in the sintering stage is finished, the temperature is increased to T2, and then heat preservation is conducted, and T1 < = T2 < = 700 DEG C; the low-temperature aging stage comprises the steps that after heat preservation in the high-temperature aging stage is finished, the temperature is reduced to T3 along with the furnace, T3 is smaller than or equal to 200 DEG C, then the temperature is increased to T4, heat preservation is conducted, and T4 is larger than or equal to T3 and smaller than or equal Cooling to room temperature along with the furnace after heat preservation in the low-temperature aging stage is finished; the chemical components of the magnet green body contain Ce, and the content of Ce is larger than or equal to 4 wt%. Rare earth cannot be separated out from the surface of the sintered neodymium-iron-boron magnet, and the yield and the magnetic performance of the magnet are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of sintered NdFeB magnets, and in particular to a sintering method of sintered NdFeB magnets and the sintered NdFeB magnets. Background Art

[0002] Compared with other magnetic materials, sintered NdFeB magnets have outstanding magnetic properties. They have extremely high magnetic energy product, coercive force and energy density, and are known as the "king of magnets". They also have good mechanical properties and are easy to process. These excellent properties have made sintered NdFeB magnets widely used in modern industry and electronic technology. The most common ones are permanent magnet motors, speakers, magnetic separators, computer disk drives, magnetic resonance imaging equipment, etc. It is composed of three elements: neodymium, iron and boron. It is made through powder metallurgy and has excellent magnetic properties, such as high coercive force, high magnetic energy product and high remanence.

[0003] However, the production cost of sintered NdFeB magnets is relatively high, mainly due to the expensive raw materials, especially the large price fluctuations of neodymium. In addition, the energy consumption and complex manufacturing process in the production process also increase the overall cost. In order to reduce costs while ensuring magnetic properties, researchers and companies are constantly exploring new alloy formulas and optimizing production processes. One of the effective cost reduction methods is to introduce a relatively cheap rare earth element, cerium (Ce), to partially replace neodymium (Nd). Cerium is not only relatively cheap, but also abundant in reserves. By adding a certain proportion of cerium to sintered NdFeB magnets, the cost of raw materials can be significantly reduced.

[0004] However, when cerium-containing magnets (Ce content ≥ 4wt%) are cooled to room temperature and then heated to the range of 520℃~540℃, a large amount of rare earth will precipitate on the surface of the magnet blank product, forming spots or spherical particles with high rare earth content. The appearance of rare earth spots or spherical particles will occupy the space between the surface of the magnet blank product and the sintering box, making it difficult to remove the magnet blank product from the sintering box, resulting in a low yield of the blank product and also having a certain impact on the performance of the blank product. Summary of the invention

[0005] Abstract: Based on the problem that a large amount of rare earth will precipitate on the surface of the sintered NdFeB magnet prepared by the current sintering process, forming spots or spherical particles with high rare earth content, the purpose of the present invention is to provide a sintering method for sintered NdFeB magnets and a sintered NdFeB magnet. The rare earth spots or spherical particles precipitated on the surface of the sintered NdFeB magnet sintered by the sintering method are effectively reduced, thereby avoiding the rare earth spots or spherical particles occupying the space between the magnet and the sintering box, improving the yield of the magnet, reducing the production cost, and avoiding the rare earth spots or spherical particles from adhering to the sintering box, so that the magnet is easy to take out from the sintering box.

[0006] The present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present application provides a sintering method for sintering NdFeB magnets, wherein the magnet green body is subjected to three stages of sintering, high temperature aging, and low temperature aging in sequence.

[0008] The sintering stage is as follows: after the magnet green body is sintered, it is cooled to T1 with the furnace and then kept warm, 300℃≤T1, and the holding time is 0.5h~10h;

[0009] The high temperature aging stage is as follows: after the sintering stage, the temperature is raised to T2 and then kept warm, T1≤T2≤950℃, and the holding time is 0.5h~10h;

[0010] The low-temperature aging stage is as follows: after the high-temperature aging stage is completed, the temperature is lowered to T3 with the furnace, T3≤200℃, and then the temperature is raised to T4 and then kept warm, T3≤T4≤500℃, and the holding time is 0.5h~10h;

[0011] After the low-temperature aging stage, the magnet is cooled to room temperature in the furnace; after the temperature of the magnet drops below 500°C, it will no longer be heated above 550°C.

[0012] The sintering temperature in the sintering stage is 1000°C to 1100°C.

[0013] Furthermore, after the high-temperature aging stage and the low-temperature aging stage are completed, the coercivity of the product is tested respectively, and then the high-temperature aging stage and the low-temperature aging stage are repeated, and then the coercivity of the product is tested again; if the difference between the two tests is within 0.3kOe, there is no need to repeat the high-temperature aging stage and the low-temperature aging stage. If the difference between the two tests is above 0.3kOe, it is necessary to repeat the high-temperature aging stage and the low-temperature aging stage until the difference between the two adjacent tests is within 0.3kOe. In actual production, the above tests are not required. The above tests are only completed in the test stage, and the final process parameters are determined through experiments.

[0014] Furthermore, the chemical composition of the magnet green body satisfies R x Fe bal M y B z ; Wherein, R is a rare earth element, M is a metal element; x represents the content of R, bal (balance) represents the content of Fe, y represents the content of M, and z represents the content of B.

[0015] Furthermore, the rare earth element R includes Ce and any one or more combinations of La, Pr, Nd, Dy, Tb, Ho, Gd, and Y.

[0016] The chemical composition of the magnet green body contains Ce, and the content of Ce is ≥4wt%.

[0017] Furthermore, the metal element M includes any one or more combinations of Al, Co, Cu, Ga, Zr, Ti, and Nb.

[0018] Further, 29wt%≤x≤33wt%, 0≤y≤3wt%, 0.88wt%≤z≤1.05wt%.

[0019] Furthermore, 500℃≤T1≤700℃.

[0020] Furthermore, 550℃≤T1≤650℃.

[0021] In a second aspect, the present application provides a sintered NdFeB magnet prepared by the above-mentioned sintering method.

[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0023] (1) The sintering method of the present application can be used to prepare sintered NdFeB magnets, which can reduce the rare earth spots or spherical particles precipitated on the surface of the sintered NdFeB magnets, so that the space between the magnets and the sintering box is more sufficient, thereby preventing the rare earth spots or spherical particles from adhering to the sintering box, making it easier to take out the magnets.

[0024] (2) The sintering method of the sintered NdFeB magnet of the present invention can improve the remanence, coercive force, intrinsic coercive force, maximum magnetic energy product and knee magnetic field of the sintered NdFeB magnet, that is, improve the overall performance of the prepared sintered NdFeB magnet;

[0025] (3) The sintering method of the sintered NdFeB magnet of the present invention can improve the yield of the sintered NdFeB magnet and reduce the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For those of ordinary skill in the art, other relevant drawings can be obtained based on these drawings without creative work. In the drawings:

[0027] Figure 1 A process flow chart of a sintering method for sintering NdFeB magnets in the present invention;

[0028] Figure 2 The effect diagram of the NdFeB magnet prepared by the sintering method of Examples 1 to 7 and Comparative Example 1 in the present invention;

[0029] Figure 3 is a temperature change curve diagram in Example 1 of the present invention;

[0030] Figure 4 is a temperature change curve diagram in Example 2 of the present invention;

[0031] Figure 5 is a temperature variation curve diagram in Example 3 of the present invention;

[0032] Figure 6 is a temperature change curve diagram in Example 4 of the present invention;

[0033] Figure 7 is a temperature variation curve diagram in Example 5 of the present invention;

[0034] Figure 8 is a temperature variation curve diagram in Example 6 of the present invention;

[0035] Fig. 9 is a temperature variation curve diagram in Example 7 of the present invention;

[0036] Fig.10 It is the temperature variation curve diagram in comparative example 1;

[0037] Fig.11 This is a line graph showing how the magnetic properties of a magnet vary with temperature. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.

[0039] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] This embodiment provides a sintering method for sintering NdFeB magnets. The sintering process is as follows: Figure 1 The formula ingredients of the magnet are shown in Table 1 below. Figure 3 Shown is the temperature change curve during the sintering process.

[0042] Table 1

[0043]

[0044]

[0045] The specific sintering method is:

[0046] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0047] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0048] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0049] The obtained green body is processed according to the following steps:

[0050] S1, sintering stage: sintering the magnet green body at 1060°C for 360 minutes, then cooling to 300°C and keeping the temperature; wherein the cooling time is 360 minutes and the keeping time is 120 minutes;

[0051] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 30 minutes and the heat preservation time is 240 minutes;

[0052] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 60 minutes and the heat preservation time is 30 minutes;

[0053] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 60 minutes and the heat preservation time is 300 minutes;

[0054] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30°C to obtain a sintered NdFeB magnet.

[0055] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0056] Example 2

[0057] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that after sintering, the temperature is lowered to 750°C in the furnace, and then heated to 900°C and then kept warm. Other process parameters are the same as those of Example 1, such as Figure 4 Shown is the temperature change curve during the sintering process.

[0058] The specific sintering method is:

[0059] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0060] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0061] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0062] The obtained green body is processed according to the following steps:

[0063] S1, sintering stage: sinter the magnet green body at 1060℃ for 360 minutes, then cool it to 750℃ and keep it warm; the cooling time is 120 minutes and the keeping time is 30 minutes;

[0064] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 900°C and then kept warm; wherein the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0065] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0066] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0067] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0068] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0069] Example 3

[0070] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that the temperature is lowered to 500°C with the furnace after sintering in the sintering stage. Other process parameters are the same as those of Example 1, such as Figure 5 Shown is the temperature change curve during the sintering process.

[0071] The specific sintering method is:

[0072] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0073] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0074] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0075] The obtained green body is processed according to the following steps:

[0076] S1, sintering stage: sintering the magnet green body at 1060℃ for 360 minutes, then cooling to 500℃ and keeping the temperature; wherein, the cooling time is 120 minutes and the keeping time is 30 minutes;

[0077] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0078] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0079] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0080] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0081] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0082] Example 4

[0083] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that after sintering, the temperature is lowered to 700°C in the furnace, and then heated to 750°C and then kept warm. Other process parameters are the same as those of Example 1, such as Figure 6 Shown is the temperature change curve during the sintering process.

[0084] The specific sintering method is:

[0085] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0086] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0087] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0088] The obtained green body is processed according to the following steps:

[0089] S1, sintering stage: sintering the magnet green body at 1060℃ for 360 minutes, then cooling to 700℃ and keeping the temperature; wherein, the cooling time is 120 minutes and the keeping time is 30 minutes;

[0090] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 750°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0091] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0092] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0093] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0094] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0095] Example 5

[0096] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that the temperature is lowered to 550°C with the furnace after sintering in the sintering stage. Other process parameters are the same as those of Example 1, such as Figure 7 Shown is the temperature change curve during the sintering process.

[0097] The specific sintering method is:

[0098] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0099] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0100] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0101] The obtained green body is processed according to the following steps:

[0102] S1, sintering stage: sinter the magnet green body at 1060℃ for 360 minutes, then cool it to 550℃ and keep it warm; the cooling time is 120 minutes and the keeping time is 30 minutes;

[0103] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0104] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0105] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0106] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0107] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0108] Example 6

[0109] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that the temperature is lowered to 580°C with the furnace after sintering in the sintering stage. Other process parameters are the same as those of Example 1, such as Figure 8 Shown is the temperature change curve during the sintering process.

[0110] The specific sintering method is:

[0111] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0112] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0113] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0114] The obtained green body is processed according to the following steps:

[0115] S1, sintering stage: sinter the magnet green body at 1060℃ for 360 minutes, then cool it to 580℃ and keep it warm; the cooling time is 120 minutes and the keeping time is 30 minutes;

[0116] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0117] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0118] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0119] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0120] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0121] Example 7

[0122] This embodiment provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that the temperature is lowered to 650°C with the furnace after sintering in the sintering stage. Other process parameters are the same as those of Example 1, such as Fig. 9 Shown is the temperature change curve during the sintering process.

[0123] The specific sintering method is:

[0124] Various raw materials are prepared according to the proportions of the elements in Table 1, and the raw materials are placed in a vacuum induction melting furnace. After melting, the sheets are thrown out to obtain quick-setting sheets.

[0125] The quick-setting sheets are subjected to hydrogen crushing and air flow milling to obtain magnetic powder.

[0126] The magnetic powder is then oriented and molded and isostatically pressed to obtain a green body.

[0127] The obtained green body is processed according to the following steps:

[0128] S1, sintering stage: sintering the magnet green body at 1060℃ for 360 minutes, then cooling to 650℃ and keeping the temperature; wherein, the cooling time is 120 minutes and the keeping time is 30 minutes;

[0129] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0130] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 30 minutes and the heat preservation time is 60 minutes;

[0131] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0132] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0133] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0134] Comparative Example 1

[0135] This comparative example provides a sintering method for sintering NdFeB magnets. The formula composition of the magnet is the same as that of Example 1. The difference from Example 1 is that the temperature is lowered to 30° C. with the furnace after sintering in the sintering stage. Other process parameters are the same as those of Example 1, such as Fig.10 Shown is the temperature change curve during the sintering process.

[0136] The specific sintering method is:

[0137] S1, sintering stage: sintering the magnet green body at 1060°C for 360 minutes, then cooling to 30°C with the furnace and keeping the temperature; wherein, the cooling time is 120 minutes and the keeping time is 30 minutes;

[0138] S2, high temperature aging stage: after the heat preservation in step S1 is completed, the temperature is raised to 700°C and then kept warm; wherein, the heating time is 240 minutes and the heat preservation time is 60 minutes;

[0139] S3, low temperature aging stage: after the heat preservation in step S2 is completed, the temperature is lowered to 100°C with the furnace and then kept warm; wherein, the cooling time is 60 minutes and the heat preservation time is 30 minutes;

[0140] S4. After the heat preservation in step S3 is completed, the temperature is raised to 420°C and then kept warm; wherein the heating time is 300 minutes and the heat preservation time is 60 minutes;

[0141] S5. After the heat preservation in step S4 is completed, the furnace is cooled to 30° C. to obtain a sintered NdFeB magnet.

[0142] The furnace cooling method during the sintering stage and the low-temperature aging stage is gas charging cooling, and the gas charged is nitrogen.

[0143] like Figure 2 As shown, it is a display diagram of the effect of the NdFeB magnets prepared by the sintering methods of Examples 1 to 7 and Comparative Example 1, from which the following information can be obtained:

[0144] Compared with Comparative Example 1, the rare earth elements precipitated on the surface of the NdFeB magnet prepared by the sintering method of Example 1 are slightly reduced.

[0145] Compared with Example 1, the rare earth elements precipitated on the surface of the NdFeB magnet prepared by the sintering method of Example 2 are significantly reduced.

[0146] Compared with Example 2, the rare earth elements precipitated on the surface of the NdFeB magnets prepared by the sintering methods of Examples 3 and 4 are more significantly reduced.

[0147] Compared with Examples 3 and 4, there is obviously no rare earth element precipitation on the surface of the NdFeB magnets prepared by the sintering methods of Examples 5-7.

[0148] The remanence (Br), coercive force (Hcb), intrinsic coercive force (Hcj), maximum magnetic energy product (BH(max)), and knee magnetic field (HK) of the NdFeB magnets prepared by the sintering methods of Examples 1 to 7 and Comparative Example 1 were tested. Three groups of samples were taken from each Example and Comparative Example for testing, and the test results are shown in Table 2 below.

[0149] Table 2

[0150]

[0151] The yield comparison of Examples 1 to 3 and Comparative Examples 1 to 3 is shown in Table 3 below.

[0152] Table 3

[0153]

[0154]

[0155] Combination Figure 2 , 11 The performance of the sintered magnet blank product prepared by the sintering method of Examples 1-7 increases with the temperature during furnace cooling, and the magnetic properties of the magnet blank product gradually increase and reach a peak. When the temperature is higher than a certain temperature value, the magnetic properties of the magnet blank product gradually decrease. Specifically:

[0156] 1. It can be seen that when the furnace holding temperature of the sintered magnet is controlled to be greater than or equal to 300°C, specifically 300°C, 500°C, 580°C, 650°C, and 700°C, the rare earth spots or spherical particles precipitated on the surface of the magnet blank product can be reduced compared with 30°C in Comparative Example 1; at the same time, various magnetic properties of the magnet blank product are higher than those in Comparative Example 1; combined with Table 3, it can be seen that the yield of the magnet blank product in Examples 1-7 is also higher than that in Comparative Example 1, which can reduce costs.

[0157] 2. Combination Figure 2 , 11When the furnace holding temperature of the sintered magnet is controlled to be 750°C, the rare earth spots or spherical particles precipitated on the surface of the magnet blank product are significantly reduced compared with Comparative Example 1, but the corresponding magnetic properties of the magnet blank product in Example 2 are lower than those in Comparative Example 1; there is the following problem: when the furnace holding temperature of the sintered magnet is controlled to be too high, although the rare earth spots or spherical particles precipitated on the surface of the magnet blank product can be significantly reduced, the magnetic properties of the magnet blank product will be significantly reduced.

[0158] On this basis, combined with 11, it can be seen that by controlling the temperature of the magnet after sintering to be within the range of 500°C-700°C during furnace cooling, the magnetic properties of the magnet are higher than those of Examples 1 and 2; at the same time, in this temperature range corresponding to Examples 3-7, combined with Figure 2 It can be seen that the rare earth spots or spherical particles precipitated from the magnet blank products prepared by the sintering method of Examples 3-7 can be further reduced on the basis of the significant reduction in Examples 1 and 2; at the same time, combined with Table 3, it can be seen that the yield of the magnet blank products in Examples 3-7 is higher than that in Examples 1 and 2.

[0159] It can be seen that by controlling the temperature of the magnet during furnace cooling after sintering within the range of 500℃-700℃, it is possible to further reduce the rare earth spots or spherical particles precipitated on the surface of the magnet blank product while ensuring that they are significantly reduced, and the magnetic properties of the magnet blank product can be higher than those in Examples 1 and 2. At the same time, the yield of the magnet blank product can be higher than that in Examples 1 and 2, which can further reduce the cost.

[0160] 3. From Fig.11 It can be seen that:

[0161] The temperature corresponding to the maximum remanence value of the magnet blank product is 550℃. When the temperature of the furnace insulation after sintering is 580℃, 650℃, 700℃ and 750℃ respectively, the remanence of the magnet blank product will gradually decrease.

[0162] The temperature corresponding to the maximum value of the intrinsic coercive force of the magnet blank product is 650°C. When the temperature of the furnace is kept warm at 700°C and 750°C respectively after sintering, the intrinsic coercive force of the magnet blank product will gradually decrease.

[0163] The temperature corresponding to the maximum coercivity of the magnet blank product is 580°C. When the temperature of the furnace is kept at 650°C, 700°C, and 750°C respectively after sintering, the coercivity of the magnet blank product will gradually decrease.

[0164] The temperature corresponding to the highest value of the maximum magnetic flux of the magnet blank product is 650°C. When the temperature of the furnace insulation after sintering is 700°C and 750°C respectively, the maximum magnetic flux of the magnet blank product will gradually decrease.

[0165] The temperature corresponding to the maximum value of the knee point magnetic field of the magnet blank product is 580℃. When the temperature of the furnace is kept warm at 650℃, 700℃ and 750℃ respectively after sintering, the knee point magnetic field of the magnet blank product will gradually decrease.

[0166] It can be seen that by controlling the temperature of the magnet after sintering to be within the range of 550°C-650°C during furnace cooling, the comprehensive magnetic properties of the magnet blank product are the strongest; at the same time, in this temperature range corresponding to Examples 5-7, combined with Figure 2 It can be seen that there are no rare earth spots or spherical particles precipitated on the surface of the magnet blank products prepared by the sintering method of Examples 5-7; at the same time, combined with Table 3, the average yield of the magnet blank products in Examples 5-7 is about 99.906%, while the average yield of the magnet blank products in Examples 3-7 is about 99.902%. It can be seen that the average yield of the magnet blank products in Examples 5-7 is higher than that in Examples 3-7, which can reduce costs to the greatest extent.

[0167] The above content proves that the sintering method of the present application can avoid the precipitation of rare earth spots or spherical particles on the surface of the magnet blank product, so that the space between the surface of the magnet blank product and the sintering box is more sufficient, avoiding the rare earth spots or spherical particles from adhering to the sintering box, making the surface of the magnet blank product easier to take out; at the same time, it can also improve the magnetic properties of the surface of the magnet blank product and improve the yield of the surface of the magnet blank product.

[0168] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A sintering method for sintering NdFeB magnets, wherein the magnet green body is subjected to three stages of sintering, high temperature aging and low temperature aging in sequence, characterized in that: The sintering stage is as follows: after the magnet green body is sintered, it is cooled to T1 with the furnace and then kept warm, 300℃≤T1; The high temperature aging stage is: after the sintering stage, the temperature is raised to T2 and then kept warm, T1≤T2≤950℃; The low-temperature aging stage is as follows: after the high-temperature aging stage is completed, the temperature is lowered to T3 with the furnace, T3≤200℃, and then the temperature is raised to T4 and then kept, T3≤T4≤500℃; After the low-temperature aging stage, the insulation is completed and the furnace is cooled to room temperature.

2. The sintering method of a sintered NdFeB magnet according to claim 1, characterized in that: After the high-temperature aging stage and the low-temperature aging stage, the coercive force of the product is tested respectively, and then the high-temperature aging stage and the low-temperature aging stage are repeated, and then the coercive force of the product is tested again; if the difference between the two tests is within 0.3kOe, there is no need to repeat the high-temperature aging stage and the low-temperature aging stage; if the difference between the two tests is above 0.3kOe, it is necessary to repeat the high-temperature aging stage and the low-temperature aging stage until the difference between the two adjacent tests is within 0.3kOe.

3. The sintering method of a sintered NdFeB magnet according to claim 1, characterized in that: The chemical composition of the magnet green body satisfies R x Fe bal M y B z ; Wherein, R is a rare earth element, M is a metal element; x represents the content of R, bal represents the content of Fe, y represents the content of M, and z represents the content of B.

4. The sintering method of a sintered NdFeB magnet according to claim 3, characterized in that: The rare earth element R includes Ce, and also includes any one or more combinations of La, Pr, Nd, Dy, Tb, Ho, Gd, and Y.

5. The sintering method of a sintered NdFeB magnet according to claim 3, characterized in that: The metal element M includes any one or more combinations of Al, Co, Cu, Ga, Zr, Ti, and Nb.

6. The sintering method of a sintered NdFeB magnet according to claim 3, characterized in that: 29wt%≤x≤33wt%, 0≤y≤3wt%, 0.88wt%≤z≤1.05wt%.

7. The sintering method of a sintered NdFeB magnet according to claim 1, characterized in that: 500℃≤T1≤700℃。 8. The sintering method of a sintered NdFeB magnet according to claim 7, characterized in that: 550℃≤T1≤650℃。 9. A sintered NdFeB magnet, characterized in that: The sintering method is used to prepare the sintering product according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • NdFeB magnet sintering method

    CN104576020A

  • Heat treatment method for improving consistency of intrinsic coercive force of neodymium iron boron blank

    CN108907203A

  • Neodymium-iron-boron magnet and preparation method thereof

    CN114334422A

  • Neodymium-iron-boron rare earth permanent magnet, preparation method therefor and use thereof

    WO2024066314A1