Surface activation bonding method and equipment
By performing surface activation treatment and applying voltage to samples with high surface roughness, the problem of low bonding strength in the surface activation bonding method is solved, and high-quality bonding under low vacuum conditions is achieved, which is suitable for polycrystalline diamond and High quality bonding of gallium oxide.
Patent Information
- Application Number
- CN202410868326.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-11
AI Technical Summary
For samples with higher surface roughness, products obtained by room temperature bonding using the surface activated bonding (SAB) method have lower bonding strengths.
By performing surface activation treatment on the first sample and the second sample, including atomic beam bombardment or plasma bombardment, the oxide film and contaminants on the sample surface are reduced, dangling bonds and surface defects on the sample surface are increased, and bias voltage and pulse voltage are applied. Room temperature bonding is performed to ensure the existence of an adsorption electric field at the interface to promote interface atomic migration and interdiffusion.
The bonding strength is significantly improved under lower vacuum conditions and is suitable for high-quality bonding of polycrystalline diamond and gallium oxide, avoiding the risk of wafer warpage and separation.
Smart Images

Figure CN118762985A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chip manufacturing, and in particular to a surface activated bonding method and equipment. Background Art
[0002] Wafer direct bonding technology (wafer bonding for short) can overcome the lattice constant mismatch between heterogeneous materials. It can achieve bonding of heterogeneous materials at low temperature or even room temperature through molecular forces or chemical bonds between the contact surfaces of heterogeneous materials. It is an important technology for heterogeneous integration.
[0003] At present, the mainstream wafer bonding methods include surface activated bonding (SAB), plasma activated bonding (PAB) and anodic bonding (AB). Both plasma activated bonding (PAB) and anodic bonding (AB) require low-temperature annealing and strengthening, and the bonded products are prone to thermal stress at the interface of heterogeneous materials, which may lead to risks such as wafer warping, bond separation and wafer fragmentation. Compared with plasma activated bonding (PAB) and anodic bonding (AB), surface activated bonding (SAB) can achieve room temperature bonding, which can avoid the occurrence of wafer warping, bond separation and wafer fragmentation, and is suitable for achieving high-quality wafer-level heterogeneous bonding. However, the use of surface activated bonding (SAB) has high requirements on the surface roughness of the wafer (Ra < 1.0nm) and needs to be in a high vacuum environment (vacuum degree < 10 -6 Therefore, for samples with high surface roughness (such as polycrystalline diamond), the bonding strength of the product obtained by room temperature bonding using the surface activated bonding (SAB) method is relatively low. Summary of the invention
[0004] The problem solved by the invention is that, for samples with high surface roughness, the bonding strength of the product obtained by room temperature bonding using a surface activated bonding (SAB) method is low.
[0005] In order to solve the above problems, the present invention provides a surface activated bonding method, comprising:
[0006] Step S1, performing surface activation treatment on the first sample and the second sample respectively to obtain a first sample to be bonded and a second sample to be bonded; wherein the surface activation treatment includes one of atomic beam bombardment and plasma bombardment;
[0007] Step S2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0008] Step S3, applying a preset pressure to the sample pair to be bonded under a preset vacuum degree, and then simultaneously applying a bias voltage and a pulse voltage between the first sample to be bonded and the second sample to be bonded to perform room temperature bonding to obtain a bonded sample pair; wherein the preset vacuum degree is not higher than 10 -2 Pa, the bias voltage is in the same direction as the pulse voltage.
[0009] Compared with the prior art, when the surface activation bonding method provided by the present invention performs room temperature bonding on samples with high surface roughness, since a bias voltage is applied between the samples to be bonded, it can ensure the existence of an adsorption electric field at the interface of the samples to be bonded, which can promote the migration and mutual diffusion of interface atoms, thereby effectively improving the bonding strength of the product; since a pulse voltage is simultaneously applied between the samples to be bonded, the surface activation bonding method can also perform room temperature bonding on samples with low conductivity. In addition, in the present invention, before room temperature bonding, by performing surface activation treatment on the sample, the oxide film and pollutants on the surface of the sample can be removed, thereby reducing the surface roughness of the sample. The reduction of the surface roughness of the sample is conducive to reducing the interfacial spacing between the samples to be bonded, thereby facilitating the improvement of the adsorption electric field at the interface, and thus facilitating the improvement of the bonding strength of the product; and, in the present invention, before room temperature bonding, by performing surface activation treatment on the sample, the atoms inside the sample can also be exposed, thereby increasing the number of dangling bonds on the surface of the sample, and at the same time, the lattice on the surface of the sample is destroyed to produce surface defects, and the surface defects can effectively capture charges to form spatial polarization charges, realize surface polarization charge retention and density improvement, thereby improving the adsorption electric field at the interface, and thus facilitating the improvement of the bonding strength of the product. It has been found through experiments that for samples with higher surface roughness, the surface activation bonding method provided by the present invention can be used to obtain products with higher bonding strength under lower vacuum conditions. Therefore, the method of the present invention can achieve high-quality bonding of polycrystalline diamond and gallium oxide.
[0010] Optionally, in step S3, the waveform of the pulse voltage includes one of a sine wave, a rectangular wave, a sawtooth wave, a triangle wave and a square wave.
[0011] Optionally, in step S3, the bias voltage is 0.1-15 kV, the amplitude of the pulse voltage is 0.05-20 kV, the frequency is 0.1-100 kHz, the pulse voltage is U, and the minimum value of U is 0.05-10 kV.
[0012] Optionally, in step S3, the room temperature bonding time is 1-60 min, and the preset pressure is 0-3 MPa.
[0013] Optionally, in step S1, the atomic beam bombardment is performed at 10 -6 -10-2 The process is carried out under a vacuum degree of 1000 Pa, the atomic beam used is an Ar atomic beam, the voltage of the atomic beam bombardment is 40-5000 V, and the bombardment time is 10-300 s.
[0014] Optionally, in step S1, the plasma bombardment is performed at 10 -6 -10 -2 Pa vacuum, and the plasma used was Ar plasma or Ar / H 2 Plasma, the voltage of the plasma bombardment is 40-5000V, and the time is 10-300s.
[0015] Optionally, the first sample is gallium nitride, and the second sample is polycrystalline diamond.
[0016] The present invention also provides a surface activation bonding device for implementing the surface activation bonding method as described above, comprising a vacuum chamber, a plasma source or a fast atom bombardment source, an upper sample stage, a lower sample stage, a driving device and a pulse bias auxiliary power supply; the plasma source or the fast atom bombardment source, the upper sample stage and the lower sample stage are all arranged in the vacuum chamber, the upper sample stage and the lower sample stage are arranged relative to each other, the driving device is used to drive at least one of the upper sample stage and the lower sample stage to move in a vertical direction; the pulse bias auxiliary power supply is used to apply bias voltage and pulse voltage.
[0017] Compared with the prior art, the device provided by the present invention can be used for samples with higher surface roughness. Experiments have found that for samples with higher surface roughness, products with higher bonding strength can be produced under lower vacuum conditions by using the device and method provided by the present invention.
[0018] Optionally, the upper sample stage and the lower sample stage are both made of dielectrics, a first electrostatic chuck electrode is disposed on the upper portion of the upper sample stage, and a second electrostatic chuck electrode is disposed on the lower portion of the upper sample stage.
[0019] Optionally, a first groove is formed on the lower end surface of the upper sample stage, and the first groove is filled with a first pressure electrode. A second groove is formed on the upper end surface of the lower sample stage, and the second groove is filled with a second pressure electrode. The first pressure electrode and the second pressure electrode are electrically connected to the pulse bias auxiliary power supply respectively. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the process of surface activated bonding method in an embodiment of the present invention;
[0021] Figure 2 It is a curve diagram when the pulse voltage waveform is a square wave in an embodiment of the present invention;
[0022] Figure 3 It is a curve diagram when the pulse voltage waveform is a sine wave in an embodiment of the present invention;
[0023] Figure 4 It is a schematic structural diagram of a surface activated bonding device in an embodiment of the present invention;
[0024] Figure 5 is a partial cross-sectional view of the upper sample stage in an embodiment of the present invention;
[0025] Figure 6 It is a partial cross-sectional view of the lower sample stage in an embodiment of the present invention.
[0026] Description of reference numerals:
[0027] 1. First sample; 2. Second sample; 3. Vacuum chamber; 4. Upper sample stage; 5. Lower sample stage; 6. Pulse bias auxiliary power supply; 7. First electrostatic chuck electrode; 8. Second electrostatic chuck electrode; 9. First pressure electrode; 10. Second pressure electrode. DETAILED DESCRIPTION
[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0029] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0030] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0031] like Figure 1 As shown, the present invention provides a surface activated bonding method, comprising:
[0032] Step S1, performing surface activation treatment on the first sample and the second sample respectively to obtain a first sample to be bonded and a second sample to be bonded; wherein the surface activation treatment includes one of atomic beam bombardment and plasma bombardment;
[0033] Step S2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0034] Step S3, applying a preset pressure to the sample pair to be bonded under a preset vacuum degree, and then simultaneously applying a bias voltage and a pulse voltage between the first sample to be bonded and the second sample to be bonded to perform room temperature bonding to obtain a bonded sample pair; wherein the preset vacuum degree is not higher than 10 -2 Pa, the bias voltage is in the same direction as the pulse voltage.
[0035] When the surface activation bonding method provided in the embodiment of the present invention performs room temperature bonding on samples with high surface roughness, since a bias voltage is applied between the samples to be bonded, it can ensure the existence of an adsorption electric field at the interface of the samples to be bonded, which can promote the migration and mutual diffusion of interface atoms, thereby effectively improving the bonding strength of the product; since a pulse voltage is simultaneously applied between the samples to be bonded, the surface activation bonding method can also perform room temperature bonding on samples with low conductivity. In addition, in the embodiment of the present invention, before room temperature bonding, the oxide film and pollutants on the surface of the sample can be removed by performing surface activation treatment on the sample, thereby reducing the surface roughness of the sample. The reduction of the surface roughness of the sample is conducive to reducing the interfacial spacing between the samples to be bonded, thereby facilitating the improvement of the adsorption electric field at the interface, and thus facilitating the improvement of the bonding strength of the product; and, in the embodiment of the present invention, before room temperature bonding, the surface activation treatment of the sample can also expose the atoms inside the sample, thereby increasing the number of dangling bonds on the surface of the sample, and also causing the lattice on the surface of the sample to be destroyed and produce surface defects, which can effectively capture charges to form spatial polarization charges, realize surface polarization charge retention and density improvement, thereby improving the adsorption electric field at the interface, and thus facilitating the improvement of the bonding strength of the product. It has been experimentally found that for samples with higher surface roughness, the surface activation bonding method provided by the embodiment of the present invention can produce products with higher bonding strength under lower vacuum conditions.
[0036] It should be noted that when performing room temperature bonding, if only a bias voltage is applied without a pulse voltage, for samples with low conductivity, the adsorption electric field at the bonding interface of the sample with low conductivity is relatively low, which will result in a lower bonding strength of the product. Therefore, the method provided in an embodiment of the present invention applies a bias voltage and a pulse voltage at the same time when performing room temperature bonding, and the method is also suitable for room temperature bonding of samples with low conductivity.
[0037] In some embodiments of the present invention, in step S3, the waveform of the pulse voltage includes one of a sine wave, a rectangular wave, a sawtooth wave, a triangle wave and a square wave.
[0038] In some embodiments of the present invention, in step S3, the bias voltage is 0.1-15 kV, the amplitude of the pulse voltage is 0.05-20 kV, the frequency is 0.1-100 kHz, the pulse voltage is U, and the minimum value of U is 0.05-10 kV.
[0039] Exemplarily, in some embodiments of the present invention, in step S3, the bias voltage is 2 kV. Figure 2As shown, the waveform of the pulse voltage is a square wave, the amplitude of the pulse voltage is 18 kV, the frequency is 1 kHz, and the minimum value of the pulse voltage is 2 kV. It should be noted that the waveform of the pulse voltage is a square wave, that is, the function satisfied by the relationship curve between the pulse voltage magnitude U and the time t is a square wave function. Figure 2 The unit of the vertical axis is kV and the unit of the horizontal axis is ms.
[0040] For example, in some embodiments of the present invention, in step S3, the bias voltage is 15 kV. Figure 3 As shown, the waveform of the pulse voltage is a sine wave, the amplitude of the pulse voltage is 10 kV, the frequency is 1 kHz, and the minimum value of the pulse voltage is 10 kV. It should be noted that the waveform of the pulse voltage is a sine wave, that is, the function satisfied by the relationship curve between the pulse voltage magnitude U and the time t is a sine function, Figure 3 The sine function is U = 15 + 5sin (2πt), Figure 3 The unit of the vertical axis is kV and the unit of the horizontal axis is ms.
[0041] In some embodiments of the present invention, in step S3, the room temperature bonding time is 1-60 min, and the preset pressure is 0-3 MPa.
[0042] In some embodiments of the present invention, in step S1, the atomic beam bombardment is performed at 10 -6 -10 -2 The process is carried out under a vacuum degree of 1.5 Pa, the atomic beam used is an Ar atomic beam, the voltage of the atomic beam bombardment is 40-100 V, and the time is 10-300 s.
[0043] In some embodiments of the present invention, in step S1, the plasma bombardment is carried out at 10 -6 -10 -2 Pa vacuum, and the plasma used was Ar plasma or Ar / H 2 Plasma, the voltage of the plasma bombardment is 40-100V, and the time is 10-300s.
[0044] In some embodiments of the present invention, the first sample is gallium nitride, and the second sample is polycrystalline diamond.
[0045] like Figure 4As shown, the present invention also provides a surface activation bonding device for realizing the surface activation bonding method as described above, comprising a vacuum chamber 3, a plasma source (not shown in the figure) or a fast atom bombardment source (not shown in the figure), an upper sample stage 4, a lower sample stage 5, a driving device (not shown in the figure) and a pulse bias auxiliary power supply 6; the plasma source or the fast atom bombardment source, the upper sample stage 4 and the lower sample stage 5 are all arranged in the vacuum chamber 3, the upper sample stage 4 and the lower sample stage 5 are arranged relative to each other, the driving device is used to drive at least one of the upper sample stage 4 and the lower sample stage 5 to move in the vertical direction; the pulse bias auxiliary power supply 6 is used to apply bias voltage and pulse voltage. The plasma source is used to generate plasma, and the fast atom bombardment source is used to generate atomic beams.
[0046] When using, Figure 4 As shown, firstly, the first sample 1 and the second sample 2 are respectively mounted on the lower end surface of the upper sample stage 4 and the upper end surface of the lower sample stage 5, and then after the vacuum chamber 3 is evacuated, the first sample 1 and the second sample 2 are surface activated by using a plasma source or a fast atom bombardment source; the upper sample stage 4 and / or the lower sample stage 5 are driven to move in the vertical direction by a driving device so that the upper sample stage 4 and the lower sample stage 5 are close to each other, and the first sample and the second sample after the surface activation treatment are aligned and attached to obtain a pair of samples to be bonded; after the vacuum chamber 3 is evacuated, the upper sample stage 4 and / or the lower sample stage 5 are driven by a driving device to apply a preset pressure to the pair of samples to be bonded, and then a bias voltage and a pulse voltage are simultaneously applied between the first sample to be bonded and the second sample to be bonded by a pulse bias auxiliary power supply 6 to perform room temperature bonding to obtain a bonded sample pair.
[0047] Compared with the prior art, the device provided by the present invention can be used for samples with higher surface roughness. Experiments have found that for samples with higher surface roughness, products with higher bonding strength can be produced under lower vacuum conditions by using the device and method provided by the present invention.
[0048] In some embodiments of the present invention, preferably, the upper sample stage 4 and the lower sample stage 5 are both made of dielectrics, a first electrostatic chuck electrode 7 is provided on the upper portion of the upper sample stage 4, and a second electrostatic chuck electrode 8 is provided on the lower portion of the upper sample stage 4; the first electrostatic chuck electrode 7 and the second electrostatic chuck electrode 8 are electrically connected to an auxiliary power supply (not shown in the figure), respectively. By applying voltage to the first electrostatic chuck electrode 7 and the second electrostatic chuck electrode 8 through the auxiliary power supply, an electrostatic attraction force can be generated between the upper sample stage 4 and the first sample 1, and between the lower sample stage 5 and the second sample 2, thereby achieving fixation of the samples.
[0049] In some embodiments of the present invention, preferably, Figure 4As shown, the lower end surface of the upper sample stage 4 is provided with a first groove, and the first groove is filled with a first pressure electrode 9. The upper end surface of the lower sample stage 5 is provided with a second groove, and the second groove is filled with a second pressure electrode 10. The first pressure electrode 9 and the second pressure electrode 10 are respectively electrically connected to the pulse bias auxiliary power supply 6. The first pressure electrode 9 and the second pressure electrode 10 serve as electrodes for applying bias voltage and pulse voltage. Figure 5 and Figure 6 As shown, the first pressure electrode 9 and the second pressure electrode 10 are both spiral-shaped.
[0050] The present invention is further described below in conjunction with specific embodiments.
[0051] Example 1
[0052] A1. Figure 4 As shown, the first sample and the second sample are fixed on the upper sample stage and the lower sample stage respectively through the first electrostatic chuck electrode and the second electrostatic chuck electrode; the vacuum chamber is evacuated to a first vacuum degree, and then the surfaces of the first sample and the second sample are bombarded with Ar atomic beams respectively to obtain the first sample to be bonded and the second sample to be bonded; wherein the first vacuum degree is 10 -6 Pa, the first sample is gallium nitride, and the second sample is polycrystalline diamond; the voltage of the Ar atomic beam bombardment is 1000V, and the time is 150s.
[0053] A2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0054] A3, evacuating the vacuum chamber to a second vacuum degree, applying a preset pressure to the sample pair to be bonded, and then simultaneously applying a bias voltage and a pulse voltage between the first sample to be bonded and the second sample to be bonded to perform room temperature bonding to obtain a bonded sample pair; wherein the second vacuum degree is 10 -6 Pa, the bonding time at room temperature is 30 min, the preset pressure is 1.5 MPa, the bias voltage is in the same direction as the pulse voltage, the bias voltage is 2 kV, and the waveform of the pulse voltage is as follows: Figure 2 For the square wave shown, the amplitude of the pulse voltage is 18 kV, the frequency is 1 kHz, and the minimum value of the pulse voltage is 2 kV.
[0055] Example 2
[0056] The difference from Example 1 is that in step A1, the first vacuum degree is 10 -2 Pa, the voltage of the Ar atomic beam bombardment is 1.5 kV, and the time is 10 s; in step A3, the second vacuum degree is 10 -2 Pa.
[0057] Example 3
[0058] The difference from Example 1 is that in step A2, a Si nano-adhesion layer is prepared on the surface of the first sample to be bonded; in step A3, when bonding is performed at room temperature, only a 2 kV bias voltage is applied, and no pulse voltage is applied.
[0059] Example 4
[0060] A1. Figure 4 As shown, the first sample and the second sample are fixed on the upper sample stage and the lower sample stage respectively through the first electrostatic chuck electrode and the second electrostatic chuck electrode; the vacuum chamber is evacuated to a first vacuum degree, and then the surfaces of the first sample and the second sample are bombarded with Ar plasma respectively to obtain the first sample to be bonded and the second sample to be bonded; wherein the first vacuum degree is 10 -2 Pa, the first sample is gallium nitride, and the second sample is polycrystalline diamond; the voltage of the Ar plasma bombardment is 1000V, and the time is 150s.
[0061] A2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0062] A3, evacuating the vacuum chamber to a second vacuum degree, applying a preset pressure to the sample pair to be bonded, and then simultaneously applying a bias voltage and a pulse voltage between the first sample to be bonded and the second sample to be bonded to perform room temperature bonding to obtain a bonded sample pair; wherein the second vacuum degree is 10 -2 Pa, the bonding time at room temperature is 30 min, the preset pressure is 1.5 MPa, the bias voltage is in the same direction as the pulse voltage, the bias voltage is 15 kV, and the waveform of the pulse voltage is as follows: Figure 3 The sine wave shown has an amplitude of 10 kV, a frequency of 1 kHz, and a minimum value of the pulse voltage of 10 kV.
[0063] Example 5
[0064] The difference from Example 4 is that in step A1, the first vacuum degree is 10 -6 Pa, the voltage of Ar plasma bombardment is 1.5 kV, and the time is 10 s; in step A3, the second vacuum degree is 10 -6 Pa.
[0065] Example 6
[0066] The difference from Example 4 is that in step A1, a Fe nano-adhesion layer is prepared on the surface of the first sample to be bonded; in step A3, when bonding is performed at room temperature, only a 15 kV bias voltage is applied, and no pulse voltage is applied.
[0067] Comparative Example 1
[0068] A1. Fix the first sample and the second sample on the upper sample stage and the lower sample stage respectively through the first electrostatic chuck electrode and the second electrostatic chuck electrode; evacuate the vacuum chamber to a first vacuum degree, and then bombard the surfaces of the first sample and the second sample with Ar atomic beams respectively to obtain a first sample to be bonded and a second sample to be bonded; wherein the first vacuum degree is 10 -6 Pa, the first sample is gallium nitride, and the second sample is polycrystalline diamond; the voltage of the Ar atomic beam bombardment is 1000V, and the time is 150s.
[0069] A2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0070] A3, evacuate the vacuum chamber to a second vacuum degree, apply a preset pressure to the sample pair to be bonded, perform room temperature bonding, and obtain a bonded sample pair; wherein the second vacuum degree is 10 -6 Pa, the bonding time at room temperature is 30 min, and the preset pressure is 1.5 MPa.
[0071] Comparative Example 2
[0072] A1. Fix the first sample and the second sample on the upper sample stage and the lower sample stage respectively through the first electrostatic chuck electrode and the second electrostatic chuck electrode; evacuate the vacuum chamber to a first vacuum degree, and then bombard the surfaces of the first sample and the second sample with Ar plasma respectively to obtain a first sample to be bonded and a second sample to be bonded; wherein the first vacuum degree is 10 - 6 Pa, the first sample is gallium nitride, and the second sample is polycrystalline diamond; the voltage of the Ar plasma bombardment is 1000V, and the time is 150s.
[0073] A2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded;
[0074] A3, evacuate the vacuum chamber to a second vacuum degree, apply a preset pressure to the sample pair to be bonded, perform room temperature bonding, and obtain a bonded sample pair; wherein the second vacuum degree is 10 -6 Pa, the bonding time at room temperature is 30 min, and the preset pressure is 1.5 MPa.
[0075] Experimental example
[0076] The tensile strength test was performed on the bonded sample pairs obtained in Examples 1-6 and Comparative Examples 1-2, and the results are shown in Table 1. It can be seen from Table 1 that the tensile strength of the bonded sample pairs obtained in Comparative Examples 1-2 is low, and the bonding fails. Compared with Comparative Examples 1-2, the tensile strength of the bonded sample pairs obtained in Examples 1-6 is greatly improved. Compared with Comparative Example 1, the tensile strength of the bonded sample pairs obtained in Example 3 is higher, and compared with Example 1-2, the tensile strength of the bonded sample pairs obtained in Example 3 is lower. Compared with Comparative Example 2, the tensile strength of the bonded sample pairs obtained in Example 6 is higher, and compared with Examples 4-5, the tensile strength of the bonded sample pairs obtained in Example 6 is lower.
[0077] Table 1
[0078]
[0079] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A surface activated bonding method, It is characterized in that include: Step S1, performing surface activation treatment on the first sample and the second sample respectively to obtain a first sample to be bonded and a second sample to be bonded; wherein the surface activation treatment includes one of atomic beam bombardment and plasma bombardment; Step S2, aligning and bonding the first sample to be bonded and the second sample to be bonded to obtain a pair of samples to be bonded; Step S3, applying a preset pressure to the pair of samples to be bonded under a preset vacuum degree, and then simultaneously applying a bias voltage and a pulse voltage between the first sample to be bonded and the second sample to be bonded to perform room temperature bonding to obtain a pair of bonded samples; wherein the preset vacuum degree is not higher than 10 -2 Pa, the bias voltage is in the same direction as the pulse voltage.
2. The surface activated bonding method according to claim 1, It is characterized in that In step S3, the waveform of the pulse voltage includes one of a sine wave, a rectangular wave, a sawtooth wave, a triangle wave and a square wave.
3. The surface activated bonding method according to claim 1, It is characterized in that In step S3, the bias voltage is 0.1-15 kV, the amplitude of the pulse voltage is 0.05-20 kV, the frequency is 0.1-100 kHz, the pulse voltage is U, and the minimum value of U is 0.05-10 kV.
4. The surface activated bonding method according to claim 3, It is characterized in that In the step S3, the room temperature bonding time is 1-60 min, and the preset pressure is 0-3 MPa.
5. The surface activated bonding method according to claim 1, It is characterized in that In step S1, the atomic beam bombards at 10 -6 -10 -2 The process is carried out under a vacuum degree of 1000 Pa, the atomic beam used is an Ar atomic beam, the voltage of the atomic beam bombardment is 40-5000 V, and the bombardment time is 10-300 s.
6. The surface activated bonding method according to claim 1, It is characterized in that In the step S1, the plasma bombardment is carried out at 10 -6 -10 -2 Pa vacuum, and the plasma used was Ar plasma or Ar / H 2 Plasma, the voltage of the plasma bombardment is 40-5000V, and the time is 10-300s.
7. The surface activated bonding method according to claim 1, It is characterized in that The first sample is gallium nitride, and the second sample is polycrystalline diamond.
8. A surface activated bonding device, It is characterized in that Used to implement the surface activated bonding method as described in any one of claims 1 to 7, comprising a vacuum chamber (3), a plasma source or a fast atom bombardment source, an upper sample stage (4), a lower sample stage (5), a driving device and a pulse bias auxiliary power supply (6); the plasma source or the fast atom bombardment source, the upper sample stage (4) and the lower sample stage (5) are all arranged in the vacuum chamber (3), the upper sample stage (4) and the lower sample stage (5) are arranged relative to each other, and the driving device is used to drive at least one of the upper sample stage (4) and the lower sample stage (5) to move in a vertical direction; the pulse bias auxiliary power supply (6) is used to apply a bias voltage and a pulse voltage.
9. The surface activated bonding device according to claim 8, It is characterized in that The upper sample stage (4) and the lower sample stage (5) are both made of dielectrics; a first electrostatic chuck electrode (7) is provided on the upper portion of the upper sample stage (4), and a second electrostatic chuck electrode (8) is provided on the lower portion of the upper sample stage (4).
10. The surface activated bonding device according to claim 9, It is characterized in that The lower end surface of the upper sample stage (4) is provided with a first groove, and the first groove is filled with a first pressure electrode (9). The upper end surface of the lower sample stage (5) is provided with a second groove, and the second groove is filled with a second pressure electrode (10). The first pressure electrode (9) and the second pressure electrode (10) are respectively electrically connected to the pulse bias auxiliary power supply (6).