GaN-HEMT device and preparation method thereof
By using caps and protective structures in the preparation process of GaN-HEMT devices, combined with wet etching technology, the problem of P-GaN surface damage is solved, the risk of gate leakage is reduced, and the reliability and control capabilities of the device are improved.
Patent Information
- Application Number
- CN202410840447.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-11
AI Technical Summary
During the preparation process of p-GaN gate HEMT devices, P-GaN surface damage often occurs, which leads to a reduction in the 2DEG concentration in the channel, weakened device gate control capabilities and gate leakage, affecting device performance.
A GaN-HEMT device and its preparation method are used, by setting a cap structure and a protective structure on the compound semiconductor composite layer, using the first and second protective structures to cover the side walls and top walls of the cap structure, combined with a wet etching process The protective structure is removed, the cap structure is exposed, the risk of surface damage is reduced, and the gate control capability is improved through dielectric layer treatment.
It effectively reduces the surface and side damage of the cap structure, reduces the risk of gate leakage, and improves the reliability and gate control capabilities of the device.
Smart Images

Figure CN118763098A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a GaN-HEMT device and a method for preparing the same. Background Art
[0002] GaN materials have high critical breakdown electric field, high electron saturation drift velocity, and AlGaN / GaN heterojunction can form high-mobility and high-density two-dimensional electron gas (2DEG), which has advantages in high-frequency, high-efficiency and high-power density applications. These characteristics determine that GaN devices have broad application prospects in power switching devices. In practical applications, normally-off GaN HEMT (high electron mobility transistor) is more popular, among which p-GaN gate HEMT devices have become the most promising candidates due to their excellent performance.
[0003] In the related art, during the preparation process of p-GaN gate HEMT devices, problems such as P-GaN surface damage often occur, which will lead to a decrease in 2DEG concentration in the channel, weakened device gate control capability, gate leakage, and ultimately affect device performance. Summary of the invention
[0004] The present application mainly provides a GaN-HEMT device and a preparation method thereof to solve the problem of P-GaN surface damage in the related art.
[0005] In order to solve the above technical problems, a technical solution adopted in the present application is to provide a GaN-HEMT device, including:
[0006] substrate;
[0007] A compound semiconductor composite layer generating a two-dimensional electron gas is arranged on the substrate;
[0008] An electrode structure, comprising: a source structure, a gate structure and a drain structure, arranged on the compound semiconductor composite layer, wherein the gate structure is located between the source structure and the drain structure;
[0009] The gate structure comprises: a cap structure disposed on the compound semiconductor composite layer and a gate metal disposed on the cap structure;
[0010] The cap structure comprises: a side wall facing the source structure and / or the drain structure;
[0011] The first protection structure extends from the surface of the compound semiconductor composite layer along the side wall in a direction away from the substrate, and the first protection structure is located between the side wall and its corresponding electrode structure.
[0012] In order to solve the above technical problems, another technical solution adopted by the present application is: to provide a method for preparing a GaN-HEMT device, comprising:
[0013] A preform of a GaN-HEMT device is provided; the preform of the GaN-HEMT device comprises a stacked substrate and a compound semiconductor composite layer generating a two-dimensional electron gas, a cap structure, a second protection structure, a first dielectric layer, a source-drain electrode layer, a second dielectric layer, and a first protection structure; wherein the source-drain electrode layer comprises a source electrode structure and a drain electrode structure arranged at intervals; the cap structure is located between the source electrode structure and the drain electrode structure, and comprises a side wall facing the source electrode structure and / or the drain electrode structure, and the first protection structure is arranged on the side wall; the second protection structure covers the top wall of the cap structure, and the first dielectric layer covers the first protection structure, the second protection structure and the compound semiconductor composite layer; the second dielectric layer covers the source electrode structure, the drain structure and the first dielectric layer;
[0014] Processing the second dielectric layer and the first dielectric layer to expose the second protective structure;
[0015] etching and removing the second protection structure by a wet etching process to expose the cap structure;
[0016] A gate metal is formed on a side of the second dielectric layer away from the first dielectric layer; the gate metal is electrically connected to the cap structure to serve as a gate structure.
[0017] The beneficial effects of the present application are as follows: Different from the prior art, the present application discloses a GaN-HEMT device and a preparation method thereof, wherein the GaN-HEMT device comprises: a substrate; a compound semiconductor composite layer generating a two-dimensional electron gas, arranged on the substrate; an electrode structure, comprising: a source structure, a gate structure and a drain structure, arranged on the compound semiconductor composite layer, the gate structure being located between the source structure and the drain structure, the gate structure comprising: a cap structure arranged on the compound semiconductor composite layer and a gate metal arranged on the cap structure; the cap structure comprising: a side wall facing the source structure and / or the drain structure; a first protective structure extending from the surface of the compound semiconductor composite layer along the side wall in a direction away from the substrate, and the first protective structure being located between the side wall and its corresponding electrode structure. Through the above arrangement, the damage to the surface and side of the cap structure can be reduced, the problem of P-GaN surface damage in the related art can be solved, the risk of gate leakage can be reduced, the gate regulation capability can be improved, and the reliability of the device can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0019] Figure 1 It is a schematic diagram of a process for preparing a GaN-HEMT device provided in one embodiment of the present application;
[0020] Figure 2 yes Figure 1 A schematic flow chart of an implementation method of step S1 in FIG.
[0021] Figure 3 yes Figure 2 Schematic diagram of the intermediate product after step S11;
[0022] Figure 4 yes Figure 2 Schematic diagram of the intermediate product after step S12;
[0023] Figure 5 yes Figure 2 A schematic flow chart of an implementation method of step S13;
[0024] Figure 6 yes Figure 5 Schematic diagram of the intermediate product after step S131;
[0025] Figure 7 yes Figure 5 Schematic diagram of the intermediate product after step S132;
[0026] Figure 8 yes Figure 5 Schematic diagram of the intermediate product after step S133;
[0027] Fig. 9 yes Figure 2 Schematic diagram of the intermediate product after step S14;
[0028] Fig.10 yes Figure 2 A schematic flow chart of an implementation method of step S15;
[0029] Fig.11 yes Fig.10 Schematic diagram of the intermediate product after step S153;
[0030] Fig.12 yes Figure 2 Schematic diagram of the intermediate product after step S16;
[0031] Fig.13 yes Figure 2 A schematic flow chart of an implementation method of step S17;
[0032] Fig.14 yes Fig.10 Schematic diagram of the intermediate product after step S171;
[0033] Fig.15 yes Fig.10 Schematic diagram of the intermediate product after step S172;
[0034] Fig.16 yes Fig.10 Schematic diagram of the intermediate product after step S173;
[0035] Fig.17 yes Figure 2 A schematic structural diagram of a preform of a GaN-HEMT device after step S18;
[0036] Fig.18 yes Figure 1 Schematic diagram of an intermediate product after the first implementation of step S2;
[0037] Fig.19 yes Figure 1 A schematic diagram of an intermediate product after the second implementation of step S2;
[0038] Fig. 20 yes Figure 1 Schematic diagram of an intermediate product after the implementation of step S3-1;
[0039] Fig.21 yes Figure 1 A schematic diagram of an intermediate product after another implementation of step S3;
[0040] Fig. 22 yes Figure 1 A schematic diagram of a product after the implementation of step S4-1;
[0041] Fig.23 yes Figure 1 Schematic diagram of the product after another implementation of step S4.
[0042] Figure Number:
[0043] GaN substrate 1; substrate 11; channel layer 12; barrier layer 13; cap layer 14; cap structure 141; second protection layer 15; second protection structure 151; second photoresist layer 16; second photoresist pattern 161; first dielectric layer 17; source opening 171; drain opening 172; first metal layer 18; source-drain layer 180; source structure 181; drain structure 182; second dielectric layer 19; gate opening 191; gate metal 20; first protection layer 21; first protection structure 211. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0045] The terms "first", "second", "third" in the embodiments of the present application are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first", "second", "third" can expressly or implicitly include at least one of the features. In the description of the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but optionally also includes steps or units that are not listed, or optionally also includes other steps or units inherent to these processes, methods, products or devices.
[0046] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0047] See also Figures 1 to 23 , Figure 1 is a schematic flow chart of a method for preparing a GaN-HEMT device provided in one embodiment of the present application, Figure 2 yes Figure 1 A schematic flow chart of an implementation method of step S1 in FIG. Figure 3 yes Figure 2 Schematic diagram of the intermediate product after step S11, Figure 4 yes Figure 2 Schematic diagram of the intermediate product after step S12, Figure 5 yes Figure 2 A schematic flow chart of an implementation method of step S13 in FIG. Figure 6 yes Figure 5 Schematic diagram of the intermediate product after step S131, Figure 7 yes Figure 5 Schematic diagram of the intermediate product after step S132, Figure 8 yes Figure 5 Schematic diagram of the intermediate product after step S133, Fig. 9 yes Figure 2 Schematic diagram of the intermediate product after step S14, Fig.10 yes Figure 2 A schematic flow chart of an implementation method of step S15 in FIG. Fig.11 yes Fig.10 Schematic diagram of the intermediate product after step S153, Fig.12 yes Figure 2 Schematic diagram of the intermediate product after step S16, Fig.13 yes Figure 2 A schematic flow chart of an implementation method of step S17 in FIG. Fig.14 yes Fig.10 Schematic diagram of the intermediate product after step S171, Fig.15 yes Fig.10 Schematic diagram of the intermediate product after step S172, Fig.16 yes Fig.10 Schematic diagram of the intermediate product after step S173, Fig.17 yes Figure 2 A schematic structural diagram of a preform of a GaN-HEMT device after step S18, Fig.18 yes Figure 1 Schematic diagram of the intermediate product after the first implementation of step S2, Fig.19 yes Figure 1 Schematic diagram of the intermediate product after the second implementation of step S2, Fig. 20 yes Figure 1 Schematic diagram of the intermediate product after the implementation of step S3, Fig.21 yes Figure 1 Schematic diagram of an intermediate product after another implementation of step S3, Fig. 22 yes Figure 1 A schematic diagram of a product after the implementation of step S4-1 in the embodiment, Fig.23 yes Figure 1 Schematic diagram of the product after another implementation of step S4.
[0048] See also Figure 1 The present application provides a method for preparing a GaN-HEMT device to prepare a GaN-HEMT device. Specifically, Figure 1 As shown, the preparation method of the GaN-HEMT device includes the following steps:
[0049] S1: providing a preform of a GaN-HEMT device; the preform of the GaN-HEMT device includes a stacked substrate 11 and a compound semiconductor composite layer that generates a two-dimensional electron gas, a cap structure 141, a second protection structure 151, a first dielectric layer 17, a source-drain layer 180, a second dielectric layer 19, and a first protection structure 211.
[0050] Specifically, a preform of a GaN-HEMT device is first provided, and the preform of the GaN-HEMT device includes a substrate 11 and a compound semiconductor composite layer that generates a two-dimensional electron gas, a cap structure 141, a second protective structure 151, a first dielectric layer 17, a source-drain layer 180, a second dielectric layer 19, and a first protective structure 211 that are sequentially stacked. In some embodiments, the compound semiconductor composite layer includes a stacked channel layer 12 and a barrier layer 13, and a two-dimensional electron gas (2DEG) is generated between the channel layer 12 and the barrier layer 13. The source-drain layer 180 includes a source structure 181 and a drain structure 182 that are spaced apart, and the source structure 181 and the drain structure 182 are both electrode structures, and the source structure 181 and the drain structure 182 are both electrically connected to the barrier layer 13 of the compound semiconductor composite layer. In a specific embodiment, the source structure 181 and the drain structure 182 are both in contact with the barrier layer 13 through vias to achieve electrical connection.
[0051] The cap structure 141 is located between the source structure 181 and the drain structure 182, and includes a sidewall facing the source structure 181 and / or the drain structure 182. In some embodiments, the cap structure 141 is a cap structure.
[0052] The first protection structure 211 is disposed on the side wall of the cap structure 141 facing the source structure 181 and / or the drain structure 182. Specifically, the first protection structure 211 extends from the surface of the compound semiconductor composite layer along the side wall of the cap structure 141 facing the source structure 181 and / or the drain structure 182 in a direction away from the substrate 11, and the first protection structure 211 is located between the side wall of the cap structure 141 and its corresponding electrode structure. In a specific embodiment, the first protection structure 211 is located between the side wall of the cap structure 141 and the source structure 181, and between the side wall of the cap structure 141 and the drain structure 182.
[0053] In a specific embodiment, the first protective structure 211 covers the side wall of the cap structure 141 and a portion of the barrier layer 13 , and the first protective structure 211 includes a first end close to the compound semiconductor composite layer and a second end away from the compound semiconductor composite layer, and the second end extends to be flush with the side of the cap structure 141 away from the substrate 11 .
[0054] The second protection structure 151 covers the top wall of the cap structure 141, and the first dielectric layer 17 covers the first protection structure 211, the second protection structure 151 and the compound semiconductor composite layer, specifically, covers the first protection structure 211, the second protection structure 151 and the barrier layer 13 of the compound semiconductor composite layer. The second dielectric layer 19 covers the source structure 181, the drain structure 182 and the first dielectric layer 17.
[0055] In a specific implementation, the step of providing a preform of a GaN-HEMT device in step S1 specifically includes:
[0056] S11: providing a GaN substrate 1; the GaN substrate 1 comprises a substrate 11, a compound semiconductor composite layer and a cap layer 14 which are stacked in sequence.
[0057] Specifically, first, a GaN substrate 1 is provided, see Figure 3 The GaN substrate 1 includes a substrate 11, a compound semiconductor composite layer and a cap layer 14 which are stacked in sequence. The compound semiconductor composite layer includes a channel layer 12 and a barrier layer 13, wherein a heterojunction structure is formed between the channel layer 12 and the barrier layer 13, and the heterojunction between the channel layer 12 and the barrier layer 13 can form a high-mobility and high-density two-dimensional electron gas.
[0058] In a specific embodiment, the material of the substrate 11 includes but is not limited to Si, SiC, etc. The material of the channel layer 12 includes GaN, and the material of the barrier layer 13 includes AlGaN, and an AlGaN / GaN heterojunction structure is formed between the channel layer 12 and the barrier layer 13 .
[0059] The cap layer 14 is a P-GaN layer, which can improve the energy band at the AlGaN / GaN heterojunction interface, making it higher than the Fermi level when the gate bias is 0V, thereby depleting the two-dimensional electron gas in the area below the gate, and facilitating the realization of normally-off characteristics. The thickness of the cap layer 14 is roughly in the range of 800A-1200A, and preferably, the thickness of the cap layer 14 is 1000A.
[0060] In other embodiments, the compound semiconductor composite layer of the GaN substrate 1 may further include a buffer layer (not shown), the buffer layer is arranged on one side of the substrate 11, the channel layer 12 and the barrier layer 13 are grown on the outer edges of the buffer layer away from the substrate 11, and the material of the buffer layer includes AlGaN.
[0061] S12 : forming a second protective layer 15 on a side of the cap layer 14 away from the compound semiconductor composite layer; the second protective layer 15 covers the cap layer 14 .
[0062] Specifically, a second protective layer 15 is formed on the side of the cap layer 14 of the GaN substrate 1 provided in step S11 away from the barrier layer 13 of the compound semiconductor composite layer, so that the second protective layer 15 covers the cap layer 14. In some embodiments, the thickness of the second protective layer 15 is greater than 3000A, and preferably, the thickness of the second protective layer 15 is in the range of 3300A-3800A.
[0063] In a specific embodiment, the step of forming the second protective layer 15 on the side of the cap layer 14 away from the compound semiconductor composite layer in step S12 specifically includes:
[0064] Si is deposited on the entire surface of the cap layer 14 away from the compound semiconductor composite layer. x O y Layer, where x>0 and y>0.
[0065] Specifically, the second protective layer 15 can be deposited on the entire surface of the barrier layer 13 of the cap layer 14 away from the compound semiconductor composite layer by any one of LPE (liquid phase deposition), MOCVD (metal organic chemical vapor deposition), HVPE (hydride vapor deposition) and MBE (molecular beam deposition), or the second protective layer 15 can be formed by inkjet printing or evaporation, so that the second protective layer 15 covers the entire surface of the cap layer 14 away from the barrier layer 13. The material of the second protective layer 15 includes Si x O y , wherein x>0 and y>0, preferably, x:y≥1:2, that is, the second protective layer 15 is Si x O y For example, the material of the second protective layer 15 may be SiO2 or Si2O3, or may be other amorphous silicon oxides. x O y The layer can be a silicon-rich material, and the silicon-rich oxide material can enhance the network structure of the material, have higher hardness and wear resistance, can improve the wear resistance or scratch resistance, and enhance the mechanical properties of the second protective layer 15, so as to better protect the cap structure 141.
[0066] In one embodiment, after step S12, the following may be formed: Figure 4 The structure shown.
[0067] S13: patterning the second protection layer 15 and the capping layer 14 to form a stacked second protection structure 151 and a capping structure 141 .
[0068] Specifically, the second protective layer 15 and the cap layer 14 are patterned to form a stacked second protective structure 151 and a cap structure 141, and the second protective structure 151 covers the cap structure 141 to protect the surface of the barrier layer 13 of the compound semiconductor composite layer away from the cap structure 141 during the preparation process, thereby reducing damage to the surface of the cap structure 141. When the second protective layer 15 and the cap layer 14 are patterned, a normal yellow light process can be used for processing. The cap layer 14 is a P-GaN layer, and the cap structure 141 obtained by patterning the cap layer 14 is also a P-GaN structure.
[0069] See also Figure 5 In a specific embodiment, the step of patterning the second protection layer 15 and the capping layer 14 in step S13 specifically includes:
[0070] S131 : forming a second photoresist layer 16 on a side of the second protection layer 15 away from the capping layer 14 .
[0071] Specifically, the second photoresist layer 16 is coated on the side of the second protective layer 15 away from the capping layer 14. Specifically, as Figure 6 As shown, a second photoresist layer 16 is coated on the surface of the second protective layer 15 away from the cap layer 14, and the second photoresist layer 16 covers the surface of the second protective layer 15 away from the cap layer 14. The second photoresist layer 16 can be a positive photoresist layer or a negative photoresist layer.
[0072] S132 : patterning the second photoresist layer 16 using a mask to form a second photoresist pattern 161 .
[0073] Specifically, the second photoresist layer 16 is a medium for pattern transfer using a photochemical reaction. Patterning the second photoresist layer 16 requires exposure, development and other steps to form a second photoresist pattern 161 .
[0074] Specifically, UV light can be used to irradiate the second photoresist layer 16 through the pattern on the mask, so that the irradiated portion of the second photoresist layer 16 undergoes a chemical reaction, and the speed at which the exposed portion of the photoresist dissolves in the developer is different from that of the unexposed portion. Therefore, after development, the pattern on the mask can be transferred to the second photoresist layer 16 to form a second photoresist pattern 161.
[0075] Among them, after the positive photoresist layer is exposed by UV light through the pattern on the mask, the exposed area undergoes photodecomposition or degradation reaction, causing the property to change, so that the exposed area can be preferentially dissolved in the positive developer, and after the development process, the unexposed part is retained to form a positive pattern, that is, forming the second photoresist pattern 161; after the negative photoresist layer is exposed by UV light through the pattern on the mask, the unexposed part can be dissolved in the negative developer, contrary to the positive photoresist layer, so that the exposed part is retained to form a negative pattern, that is, forming the second photoresist pattern 161. In a specific embodiment, after step S132, the following can be formed. Figure 7 The structure shown.
[0076] S133 : etching by dry etching to remove the portion of the second protection layer 15 and the portion of the capping layer 14 that are not covered by the second photoresist pattern 161 .
[0077] Specifically, after the second photoresist layer 16 is patterned and the second photoresist pattern 161 is formed, the second photoresist pattern 161 is used as a barrier layer, and the second protective layer 15 and the cap layer 14 are etched using a dry etching process to complete the patterning of the second protective layer 15 and the cap layer 14, thereby forming a stacked second protective structure 151 and a cap structure 141.
[0078] In one embodiment, the second protective layer 15 is Si x O y The Si layer can be etched by an inductively coupled plasma (ICP) etching process, with the second photoresist pattern 161 as a barrier layer. x O y The layer and the capping layer 14 are etched to remove the portion of the second protective layer 15 and the portion of the capping layer 14 not covered by the second photoresist pattern 161, and retain the portion of the second protective layer 15 and the portion of the capping layer 14 covered by the second photoresist pattern 161 to form a second protective structure 151 and a capping structure 141.
[0079] Specifically, after removing the portion of the second protective layer 15 and the portion of the cap layer 14 not covered by the second photoresist pattern 161 to form the second protective structure 151 and the cap structure 141, it is also necessary to remove the second photoresist pattern 161 covering the second protective structure 151 so that the second protective structure 151 is exposed.
[0080] In a specific embodiment, the projections of the second protection structure 151 and the cap structure 141 on the barrier layer 13 overlap, that is, the second protection structure 151 only covers the surface of the cap structure 141 away from the barrier layer 13. After step S133, the following can be formed: Figure 8 The structure shown.
[0081] In other embodiments, the projection of the cap structure 141 on the barrier layer 13 may also be located within the projection of the second protective structure 151 on the barrier layer 13 of the compound semiconductor composite layer, that is, the second protective structure 151 may partially cover the surface of the cap structure 141 away from the barrier layer 13, and the other part may extend to the surface of the barrier layer 13 away from the channel layer 12.
[0082] S14: forming a first protective layer 21 on a side of the second protective structure 151 away from the compound semiconductor composite layer; the first protective layer 21 covers the second protective structure 151 and the compound semiconductor composite layer.
[0083] Specifically, the first protective layer 21 is formed on the side of the second protective structure 151 away from the barrier layer 13 of the compound semiconductor composite layer, so that the first protective layer 21 covers the second protective structure 151 and the barrier layer 13 of the compound semiconductor composite layer, and the first protective layer 21 covers the side wall of the cap structure 141. In some embodiments, the thickness of the first protective layer 21 is approximately in the range of 800A-1200A, preferably, the thickness of the first protective layer 21 is 1000A, and the thickness of the first protective layer 21 is approximately equal to the thickness of the cap structure 141, so as to better contact with the surface of the barrier layer 13 and the side wall of the cap structure 141.
[0084] In a specific embodiment, the step of forming the first protective layer 21 on the side of the second protective structure 151 away from the compound semiconductor composite layer in step S14 specifically includes:
[0085] Si is deposited on the entire surface of the second protection structure 151 away from the compound semiconductor composite layer and the surface of the compound semiconductor composite layer away from the substrate 11. x O y Layer, where x>0 and y>0.
[0086] Specifically, the first protective layer 21 can be deposited on the surface of the barrier layer 13 of the second protective structure 151 away from the compound semiconductor composite layer and the surface of the barrier layer 13 of the compound semiconductor composite layer away from the substrate 11 by any one of LPE (liquid phase deposition), MOCVD (metal organic chemical vapor deposition), HVPE (hydride vapor deposition) and MBE (molecular beam deposition). The first protective layer 21 can also be formed by inkjet printing or evaporation, so that the surface of the second protective structure 151 away from the barrier layer 13 and the surface of the barrier layer 13 away from the substrate 11 are covered by the first protective layer 21. The material of the first protective layer 21 includes Si x O y , wherein x>0 and y>0, preferably, x:y≥1:2, that is, the first protective layer 21 is Si x Oy For example, the material of the first protective layer 21 may be SiO2 or Si2O3, or may be other amorphous silicon oxides. x O y The layer can be a silicon-rich material, and the silicon-rich oxide material can enhance the network structure of the material, have higher hardness and wear resistance, can improve the wear resistance or scratch resistance, and improve the mechanical properties of the first protective layer 21, so as to better protect the cap structure 141. The material of the first protective layer 21 and the material of the second protective layer 15 can be the same or different.
[0087] In one embodiment, after step S14, the following may be formed: Fig. 9 The structure shown.
[0088] S15 : patterning the first protection layer 21 to form a first protection structure 211 .
[0089] Specifically, the first protective layer 21 is patterned to form a first protective structure 211 disposed on the side wall of the cap structure 141. The first protective structure 211 may completely cover the side wall of the cap structure 141, or may partially cover the side wall of the cap structure 141. Preferably, the first protective structure 211 completely covers the side wall of the cap structure 141. The first protective structure 211 includes a first end close to the compound semiconductor composite layer and a second end away from the compound semiconductor composite layer. The second end extends to be flush with the side of the cap structure 141 away from the substrate 11. Since the first protective structure 211 covers the side wall of the cap structure 141, the side of the cap structure 141 can be protected during the preparation process to reduce damage to the side of the cap structure 141. When the first protective layer 21 is patterned, a normal yellow light process can be used for processing.
[0090] See also Fig.10 In a specific embodiment, the step of patterning the first protective layer 21 to form the first protective structure 211 in step S15 specifically includes:
[0091] S151 : forming a first photoresist layer on a side of the first protective layer 21 away from the compound semiconductor composite layer.
[0092] Specifically, a first photoresist layer (not shown) is coated on the surface of the barrier layer 13 of the compound semiconductor composite layer away from the first protective layer 21, and the first photoresist layer covers the surface of the barrier layer 13 of the first protective layer 21 away from the compound semiconductor composite layer. The first photoresist layer can be a positive photoresist layer or a negative photoresist layer.
[0093] S152: patterning the first photoresist layer using a mask to form a first photoresist pattern.
[0094] Specifically, the first photoresist layer is patterned, and it is necessary to form a first photoresist pattern (not shown) through exposure, development and other steps. The specific method of patterning the first photoresist layer can refer to the method of patterning the second photoresist layer 16 using a mask in S132, which will not be repeated here. After the first photoresist layer is patterned using a mask, a first photoresist pattern can be formed.
[0095] S153: removing the portion of the first protection layer 21 not covered by the first photoresist pattern by dry etching.
[0096] Specifically, after the first photoresist layer is patterned and the first photoresist pattern is formed, the first photoresist pattern is used as a barrier layer and the first protective layer 21 is etched using a dry etching process to complete the patterning of the first protective layer 21, thereby forming a first protective structure 211 arranged on the side wall of the cap structure 141.
[0097] Specifically, after removing the portion of the first protection layer 21 not covered by the first photoresist pattern to form the first protection structure 211 , it is also necessary to remove the first photoresist pattern covering the first protection structure 211 to expose the first protection structure 211 .
[0098] In a specific implementation, after step S153, the following may be formed: Fig.11 Specifically, the second end of the first protection structure 211 away from the compound semiconductor composite layer extends to be flush with the side of the cap structure 141 away from the substrate 11, the width of the first end of the first protection structure 211 close to the compound semiconductor composite layer is greater than the width of the second end away from the compound semiconductor composite layer, and the side of the first protection structure 211 away from the cap structure 141 is a curved surface.
[0099] S16: forming a first dielectric layer 17 on a side of the second protection structure 151 away from the compound semiconductor composite layer.
[0100] Specifically, a first dielectric layer 17 is formed on a side of the second protective structure 151 away from the barrier layer 13 of the compound semiconductor composite layer. In a specific embodiment, the first dielectric layer 17 can be deposited on a side of the second protective structure 151 away from the barrier layer 13 by using any deposition method such as chemical vapor deposition (CVD) or physical vapor deposition (PVD). Alternatively, the first dielectric layer 17 can be formed on a side of the second protective structure 151 away from the barrier layer 13 by using inkjet printing or evaporation.
[0101] In a specific embodiment, the material of the first dielectric layer 17 includes Si a N b, wherein a>0 and b>0, preferably, a:b≥3:4, the step of forming the first dielectric layer 17 on the side of the second protection structure 151 away from the compound semiconductor composite layer in step S16 comprises:
[0102] Full surface deposition of Si a N b layer.
[0103] Specifically, Si is deposited on the entire surface of the second protection structure 151 away from the barrier layer 13. a N b Layer, Si a N b The barrier layer 13 covering the first protection structure 211 and the second protection structure 151 and the surface of the compound semiconductor composite layer away from the channel layer 12. The material of the first dielectric layer 17 includes Si a N b , where Si a N b It can be Si3N4 or other amorphous silicon nitride compounds. The material of the first dielectric layer 17 is Si a N b The first dielectric layer 17 can supplement the surface of the barrier layer 13, i.e., the AlGaN layer, with N elements, thereby adjusting the two-dimensional electron gas and playing a repairing role. a N b The layer is nitrogen-rich material, which can improve Si a N b Materials and Si x O y The material's etching selectivity makes it easier to achieve etching morphology in subsequent processes.
[0104] In some embodiments, the thickness of the deposited first dielectric layer 17 is in the range of 1000A-1500A. Preferably, the thickness of the first dielectric layer 17 is 1250A. In a specific embodiment, after step S16, the following may be formed: Fig.12 The structure shown.
[0105] S17 : forming a source-drain electrode layer 180 on a side of the first dielectric layer 17 away from the compound semiconductor composite layer; wherein the thickness of the second protective layer 15 is greater than the thickness of the source-drain electrode layer 180 .
[0106] Specifically, a source-drain layer 180 is formed on the side of the first dielectric layer 17 away from the barrier layer 13 of the compound semiconductor composite layer. The source-drain layer 180 includes a source structure 181 and a drain structure 182 that are spaced apart, and both the source structure 181 and the drain structure 182 are electrically connected to the barrier layer 13 of the compound semiconductor composite layer.
[0107] See also Fig.13 In a specific embodiment, the step of forming the source-drain electrode layer 180 on the side of the first dielectric layer 17 away from the compound semiconductor composite layer in step S17 specifically includes:
[0108] S171 : forming a source opening 171 and a drain opening 172 on the first dielectric layer 17 .
[0109] Specifically, the first dielectric layer 17 may be patterned by a normal yellow light process, by coating a photoresist on the first dielectric layer 17, using UV light to irradiate through the pattern on the mask, performing an exposure process, and after development, the first dielectric layer 17 is etched by an etching process to form a source opening 171 and a drain opening 172 spaced apart from each other on the first dielectric layer 17. In one embodiment, the first dielectric layer 17 may be etched by an inductively coupled plasma etching process to form the source opening 171 and the drain opening 172. After the etching is completed, the remaining photoresist needs to be removed to expose the surface of the first dielectric layer 17 away from the barrier layer 13.
[0110] Specifically, the surface of the barrier layer 13 of the compound semiconductor composite layer away from the channel layer 12 is exposed through the source opening 171 and the drain opening 172 at the position corresponding to the source opening 171 and the drain opening 172, that is, the source opening 171 and the drain opening 172 are through holes formed on the first dielectric layer 17, and the source opening 171 and the drain opening 172 both penetrate the first dielectric layer 17. The source opening 171 and the drain opening 172 are respectively arranged at opposite sides of the cap structure 141. In one embodiment, after step S171, the following can be formed: Fig.14 The structure shown.
[0111] S172 : Depositing a first metal layer 18 on a surface of the first dielectric layer 17 away from the compound semiconductor composite layer.
[0112] Specifically, the first metal layer 18 can be deposited on the surface of the barrier layer 13 of the first dielectric layer 17 away from the compound semiconductor composite layer by any deposition method of chemical vapor deposition or physical vapor deposition, or the first metal layer 18 can be deposited on the surface of the first dielectric layer 17 away from the barrier layer 13 by inkjet printing or evaporation. Part of the first metal layer 18 fills the source opening 171 and the drain opening 172, and contacts the surface of the barrier layer 13 away from the channel layer 12, and the other part covers the surface of the first dielectric layer 17 away from the barrier layer 13. In some embodiments, the thickness of the first metal layer 18 is approximately in the range of 2800A-3200A, and preferably, the thickness of the first metal layer 18 is 3000A. The thickness of the first metal layer 18 is smaller than the thickness of the second protection structure 151, so that the height of the second protection structure 151 away from the surface of the barrier layer 13 is higher than the height of the first metal layer 18 away from the surface of the barrier layer 13, thereby avoiding the influence on the first metal layer 18, i.e., the source and drain layer 180, when the first dielectric layer 17 on the top of the second protection structure 151 is processed in the subsequent process.
[0113] In one embodiment, after step S172, the following may be formed: Fig.15 The structure shown.
[0114] S173 : patterning the first metal layer 18 .
[0115] Specifically, the first metal layer 18 can be patterned by a normal photolithography process, and the first metal layer 18 corresponding to the source opening 171 and the drain opening 172 is retained to form a source structure 181 and a drain structure 182 spaced apart at positions corresponding to the source opening 171 and the drain opening 172, so as to prepare a source-drain layer 180. The source structure 181 is electrically connected to the barrier layer 13 through the source opening 171, and the drain structure 182 is electrically connected to the barrier layer 13 through the drain opening 172. The first protection structure 211 is located between the side wall of the cap structure 141 and its corresponding electrode structure. Specifically, the first protection structure 211 is located between the side wall of the cap structure 141 and the source structure 181 and between the side wall of the cap structure 141 and the drain structure 182. The width direction of the first protection structure 211 is the arrangement direction of the source structure 181 and the drain structure 182. The side of the first protection structure 211 facing the source structure 181 and / or the drain structure 182 is a curved surface.
[0116] The specific process steps of the yellow light process can refer to the steps of patterning the second protective layer 15 and the capping layer 14 described in step S13 or the prior art, which will not be described in detail here. In one embodiment, after step S173, the following can be formed: Fig.16 The structure shown.
[0117] S18: forming a second dielectric layer 19 on a side of the source / drain electrode layer 180 away from the compound semiconductor composite layer.
[0118] Specifically, the second dielectric layer 19 can be formed on the side of the source and drain layer 180 away from the barrier layer 13 of the compound semiconductor composite layer by using any deposition method such as chemical vapor deposition or physical vapor deposition. Alternatively, the second dielectric layer 19 can be formed on the side of the source and drain layer 180 away from the barrier layer 13 by using inkjet printing or evaporation.
[0119] In a specific embodiment, the material of the second dielectric layer 19 includes Si a N b , wherein a>0 and b>0, the step of forming the second dielectric layer 19 on the side of the source-drain electrode layer 180 away from the compound semiconductor composite layer in step S18 comprises:
[0120] Full surface deposition of Si a N b layer.
[0121] Specifically, the material of the second dielectric layer 19 includes Si a N b , the second dielectric layer 19 is Si a N b Layer, a>0 and b>0, preferably, a:b≥3:4, Si is deposited on the entire surface of the source and drain layer 180 away from the barrier layer 13 a N b Layer, Si a N b The source structure 181 and the drain structure 182 of the source-drain layer 180 are covered away from the surface of the channel layer 12 and the surface of the first dielectric layer 17 is away from the channel layer 12. The second dielectric layer 19 is a passivation layer, which can facilitate the subsequent ion implantation process, and can also adjust the voltage resistance of the device, and serve as a protective layer for device isolation to isolate the active area and the passive area of the device.
[0122] In some embodiments, Si a N b It can be Si3N4 or other amorphous silicon nitride compounds. The material of the second dielectric layer 19 and the first dielectric layer 17 can be the same or different. Preferably, the material of the second dielectric layer 19 and the first dielectric layer 17 is the same, so that the second dielectric layer 19 and the first dielectric layer 17 can be processed simultaneously in the subsequent process. In some embodiments, the second dielectric layer 19 is Si a N b The layer is nitrogen-rich material, which can improve Si a N b Materials and Si x O yThe material's etching selectivity makes it easier to achieve etching morphology in subsequent processes.
[0123] In some embodiments, the thickness of the second dielectric layer 19 is greater than 2000 Å. Preferably, the thickness of the second dielectric layer 19 is in the range of 2300 Å-2800 Å.
[0124] In a specific embodiment, after step S18, the following may be formed: Fig.17 The preform structure of the GaN-HEMT device is shown.
[0125] S2: Process the second dielectric layer 19 and the first dielectric layer 17 to expose the second protection structure 151 .
[0126] Specifically, the second dielectric layer 19 and the first dielectric layer 17 are processed to remove the second dielectric layer 19 and the first dielectric layer 17 covering the second protective structure 151 , so that the second protective structure 151 is exposed.
[0127] In the first embodiment, the step of processing the second dielectric layer 19 and the first dielectric layer 17 to expose the second protection structure 151 in step S2 specifically includes:
[0128] The second dielectric layer 19 is planarized by chemical mechanical polishing to remove the portion of the first dielectric layer 17 covering the second protection structure 151 and make the surface of the second dielectric layer 19 away from the substrate 11 flat, exposing the second protection structure 151 .
[0129] Specifically, the second dielectric layer 19 may be planarized by using a chemical mechanical polishing (CMP) process, and a portion of the second dielectric layer 19 may be removed, so that the surface of the second dielectric layer 19 away from the substrate 11 is formed into a plane, and at the same time, the portion of the first dielectric layer 17 covering the second protective structure 151 is removed, so that the second protective structure 151 is exposed, and the surface of the second protective structure 151 away from the barrier layer 13 is flush with the surface of the second dielectric layer 19 away from the barrier layer 13. That is, in the process of planarizing the second dielectric layer 19 by using chemical mechanical polishing, the portion of the first dielectric layer 17 covering the second protective structure 151 is removed, so that the second protective structure 151 is exposed.
[0130] Since the thickness of the second protection structure 151 is greater than the thickness of the source-drain electrode layer 180, the surface of the second protection structure 151 away from the barrier layer 13 is higher than the surface of the source-drain electrode layer 180 away from the barrier layer 13, and during the polishing process of the chemical mechanical polishing process, one type of grinding liquid can only grind one type of material, therefore, even if the first dielectric layer 17 and the second dielectric layer 19 are ground to expose the second protection structure 151, the source-drain electrode layer 180 and the second protection structure 151 will not be ground, and the influence on the source-drain electrode layer 180 and the second protection structure 151 during the chemical mechanical polishing process can be avoided. Moreover, the planarization process of the second dielectric layer 19 by the chemical mechanical polishing process can simplify the yellow light and etching process in the subsequent process, that is, because the surface of the second dielectric layer 19 is flat, it does not need excessive exposure and development, that is, over-etching, and the problem of dielectric sidewall thinning caused by the height difference of dielectric deposition can be avoided, which can effectively reduce gate leakage and improve gate control ability, thereby improving device reliability.
[0131] In this embodiment, after step S2, the following can be obtained: Fig.18 The structure shown.
[0132] In the second embodiment, the step of processing the second dielectric layer 19 and the first dielectric layer 17 to expose the second protection structure 151 in step S2 specifically includes:
[0133] The second dielectric layer 19 and the first dielectric layer 17 are etched by a dry etching process to expose the second protection structure 151 .
[0134] Specifically, in this embodiment, the step of etching the second dielectric layer 19 and the first dielectric layer 17 by dry etching to expose the second protection structure 151 specifically includes:
[0135] The second dielectric layer 19 and the first dielectric layer 17 are etched using inductively coupled plasma.
[0136] Specifically, the second dielectric layer 19 and the first dielectric layer 17 are etched by an inductively coupled plasma etching process to etch away portions of the first dielectric layer 17 and the second dielectric layer 19 corresponding to the second protective structure 151, and a gate opening 191 is formed on the first dielectric layer 17 and the second dielectric layer 19, so that the surface of the second protective structure 151 away from the barrier layer 13 is exposed through the gate opening 191.
[0137] In some embodiments, since the materials of the second dielectric layer 19 and the first dielectric layer 17 both include Si a N b , a>0 and b>0, preferably, a:b≥3:4, the first dielectric layer 17 and the second dielectric layer 19 are both Si a N blayer, the material of the second protective structure 151 is Si x O y , x>0 and y>0, preferably, x:y≥1:2, due to the inductively coupled plasma etching process, Si a N b Material rate and etching Si x O y The rates of the materials are similar, therefore, the second dielectric layer 19 and the first dielectric layer 17 can be etched in a fixed time (by time) manner. By etching in a by time manner and controlling the etching time, the etching effect on the second dielectric layer 19 and the first dielectric layer 17 can be ensured. At the same time, it can also be avoided that the dry etching time is too long to partially or completely etch away the second protection structure 151, affecting the protection effect of the second protection structure 151 on the cap structure 141, causing damage to the surface of the cap structure 141 during the dry etching (plasma bombardment) process, thereby causing the gate control capability to be weakened or failed, resulting in the problem of gate leakage, which is beneficial to improving the reliability of the prepared device.
[0138] Specifically, in this embodiment, after step S2, the following can be formed: Fig.19 The structure shown.
[0139] S3: removing the second protection structure 151 by wet etching to expose the capping structure 141 .
[0140] Specifically, in one embodiment, the step of removing the second protection structure 151 by a wet etching process to expose the cap structure 141 in step S3 specifically includes:
[0141] The second protection structure 151 is etched using a buffered oxide etching solution (BOE solution).
[0142] Specifically, a buffered oxide etchant is used to etch the second protective structure 151, wherein the etching rate of the buffered oxide etchant on the second protective structure 151 is greater than the etching rate of the second dielectric layer 19 and the first dielectric layer 17, so as to avoid the buffered oxide etchant etching the second dielectric layer 19 and the first dielectric layer 17 at too fast a rate, resulting in the second protective structure 151 not being etched away while the second dielectric layer 19 and the first dielectric layer 17 have been etched, causing the surface of the cap structure 141 to be damaged.
[0143] In one embodiment, the materials of the second dielectric layer 19 and the first dielectric layer 17 are both Si a N b The material of the second protection structure 151 is Si x O y, x>0 and y>0, a>0 and b>0, preferably, a:b≥3:4, x:y≥1:2, the components of the buffered oxide etchant include NH4F and HF. The volume ratio of NH4F to HF in the buffered oxide etchant is in the range of 3:1-8:1, and in a preferred embodiment, the volume ratio of NH4F to HF in the buffered oxide etchant is 5:1.
[0144] Specifically, the second protection structure 151, ie, Si x O y When the material is added, the reaction equation is as follows:
[0145] Formula 1:Si x O y +zHF→H x [SiF z ]+H z-x O y ;
[0146] Formula 2: NH4F→NH3↑+HF;
[0147] After the above reaction, the second protective structure 151, namely Si x O y The material is etched away by the buffered oxide etchant, so that the cap structure 141 is exposed.
[0148] Under the same etching conditions, there is an etching selectivity ratio between different materials. In the embodiment of the present application, the buffered oxide etching solution has a selectivity ratio of 0.04 to 0.06. a N b Materials and Si x O y The etching rates of the materials are different. In some embodiments, the buffered oxide etchant etches Si a N b The material rate is in the range of 400A / min-600A / min, and the buffered oxide etchant etches Si x O y The material rate is within the range of 1500A / min-2000A / min, and the concentration and temperature of the original solution can be adjusted to achieve the desired effect. In a preferred embodiment, the buffered oxide etching solution etches Si a N b The material rate is 500A / min, and the buffered oxide etchant etches Si x O y The material rate is 1800 A / min to ensure the best etching effect on the second protection structure 151 .
[0149] In one embodiment, step S2 uses a chemical mechanical polishing process to planarize the second dielectric layer 19, so that the second dielectric layer 19 is a flat layer and the second protection structure 151 is exposed. When the second protection structure 151 is removed by a wet etching process in step S3, the second protection structure 151 is removed, and a gate opening 191 is formed at a position of the second dielectric layer 19 corresponding to the cap structure 141, so that the surface of the second protection structure 151 away from the barrier layer 13 is exposed through the gate opening 191. In this embodiment, after step S3, the second protection structure 151 is etched away, and the following can be formed. Fig. 20 The structure shown.
[0150] In another embodiment, step S2 uses a dry etching process to etch the second dielectric layer 19 and the first dielectric layer 17, and a gate opening 191 corresponding to the second protection structure 151 is formed in the second dielectric layer 19 and the first dielectric layer 17. The second protection structure 151 is exposed through the gate opening 191. After step S3, the second protection structure 151 is etched away, and the following can be formed: Fig.21 The structure shown.
[0151] S4: forming a gate metal 20 on a side of the second dielectric layer 19 away from the first dielectric layer 17 , and the gate metal 20 is electrically connected to the cap structure 141 to serve as a gate structure.
[0152] Specifically, the second metal layer (not shown) can be deposited on the surface of the second dielectric layer 19 away from the first dielectric layer 17 by any deposition method of chemical vapor deposition or physical vapor deposition, or the second metal layer can be deposited on the surface of the second dielectric layer 19 away from the first dielectric layer 17 by inkjet printing or evaporation. Part of the second metal layer fills the gate opening 191 and contacts the surface of the cap structure 141 away from the barrier layer 13 to achieve electrical connection, and the other part covers the surface of the second dielectric layer 19 away from the first dielectric layer 17. Then, the second metal layer is etched by a normal yellow light process, and the part of the second metal layer corresponding to the cap structure 141 is retained, and the rest of the part is etched to prepare the gate metal 20. The gate metal 20 is electrically connected to the cap structure 141 as a gate structure, and the gate structure and the source structure 181 and the drain structure 182 are all electrode structures.
[0153] The specific process steps of the yellow light process can refer to the steps of patterning the second protective layer 15 and the capping layer 14 described in step S13 or the prior art, which will not be described in detail here.
[0154] In one embodiment, the second dielectric layer 19 is a flat layer, and the gate opening 191 is formed in the second dielectric layer 19. After step S4, the following can be formed: Fig. 22The structure shown in FIG. 1 is a GaN-HEMT device. That is, by using the method for preparing the GaN-HEMT device provided in this embodiment, a GaN-HEMT device can be prepared as shown in FIG. Fig. 22 The GaN-HEMT device shown.
[0155] In another embodiment, the second dielectric layer 19 is a non-planar layer, and the gate opening 191 is formed in the second dielectric layer 19 and the first dielectric layer 17. After step S4, the following can be formed: Fig.23 The structure shown in FIG. 1 is a GaN-HEMT device. That is, by using the method for preparing the GaN-HEMT device provided in this embodiment, a GaN-HEMT device can be prepared as shown in FIG. Fig.23 The GaN-HEMT device shown.
[0156] In the present application, a GaN-HEMT device is prepared by adopting the above-mentioned preparation method of the GaN-HEMT device, and a cap structure 141 is formed on the barrier layer 13 of the compound semiconductor composite layer, so as to improve the energy band at the AlGaN / GaN heterojunction interface, thereby facilitating the realization of the normally-off characteristics of the GaN-HEMT device; a second protection structure 151 is formed on a side of the cap structure 141 away from the barrier layer 13 of the compound semiconductor composite layer, and a first protection structure 211 is formed on the side wall of the cap structure 141 facing the source structure 181 and / or the drain structure 182, and the first dielectric layer 17 and the second dielectric layer 19 are covered on the second protection structure 151. The first dielectric layer 17 and the second dielectric layer 19 are firstly processed to expose the second protection structure 151, for example, by chemical mechanical polishing. The process flattens the second dielectric layer 19 or etches the first dielectric layer 17 and the second dielectric layer 19 by a dry etching process; then, the second protective structure 151 is etched by a wet etching process. When the first dielectric layer 17 and the second dielectric layer 19 are processed, the second protective structure 151 can protect the surface of the barrier layer 13 of the cap structure 141 away from the compound semiconductor composite layer, and the first protective structure 211 can protect the side wall of the cap structure 141 to avoid damage to the upper surface or side of the cap structure 141 during plasma bombardment when etching the first dielectric layer 17 and the second dielectric layer 19. At the same time, it also avoids directly etching the second protective structure 151 by a dry etching process and causing damage to the surface of the cap structure 141, resulting in weakened or even failed gate control capability and gate leakage.
[0157] Wet etching has the advantages of simple equipment, low cost, and high selectivity. Its isotropic characteristics can also effectively solve the device damage caused by plasma during dry etching. The second protection structure 151 and the first dielectric layer 17 and the second dielectric layer 19 are made of different materials. The second protection structure 151 is etched by utilizing the etching selectivity between different materials under the same etching conditions. A GaN-HEMT device with low surface damage of the cap structure 141 can be obtained, which can effectively reduce the risk of gate leakage and enhance the gate control capability, thereby improving device reliability.
[0158] See also Fig. 22 and Fig.23 The present application also provides a GaN-HEMT device, which can be prepared by using any of the preparation methods of the GaN-HEMT device provided in the present application.
[0159] Specifically, the GaN-HEMT device includes a substrate 11, a compound semiconductor composite layer generating a two-dimensional electron gas, an electrode structure and a first protective structure 211. The compound semiconductor composite layer is disposed on the substrate 11, the electrode structure is disposed on the compound semiconductor composite layer, the electrode structure includes a source structure 181, a gate structure and a drain structure 182, the gate structure is located between the source structure 181 and the drain structure 182, wherein the gate structure includes a cap structure 141 disposed on the compound semiconductor composite layer and a gate metal 20 disposed on the cap structure 141. The cap structure 141 includes a side wall facing the source structure 181 and / or the drain structure 182, the first protective structure 211 extends from the surface of the compound semiconductor composite layer along the side wall of the cap structure 141 facing the source structure 181 and / or the drain structure 182 in a direction away from the substrate 11, and the first protective structure 211 is located between the side wall of the cap structure 141 and its corresponding electrode structure.
[0160] In a specific embodiment, the first protection structure 211 is located between the sidewall of the cap structure 141 facing the source structure 181 and the source structure 181 , and between the sidewall of the cap structure 141 facing the drain structure 182 and the drain structure 182 .
[0161] In some embodiments, the compound semiconductor composite layer includes a stacked channel layer 12 and a barrier layer 13, a heterojunction structure is formed between the channel layer 12 and the barrier layer 13, and the heterojunction between the channel layer 12 and the barrier layer 13 can form a high-mobility and high-density two-dimensional electron gas.
[0162] In a specific embodiment, the material of the substrate 11 includes but is not limited to Si, SiC, etc. The material of the channel layer 12 includes GaN, and the material of the barrier layer 13 includes AlGaN, and an AlGaN / GaN heterojunction structure is formed between the channel layer 12 and the barrier layer 13 .
[0163] In one embodiment, the cap structure 141 is a P-GaN structure, and the cap structure 141 is disposed on the side of the barrier layer 13 away from the substrate 11. The cap structure 141 can increase the energy band at the AlGaN / GaN heterojunction interface, and make it higher than the Fermi level when the gate bias is 0V, thereby depleting the two-dimensional electron gas in the area below the gate, so as to facilitate the realization of the normally-off characteristic. The thickness of the cap structure 141 is approximately in the range of 800A-1200A, and preferably, the thickness of the cap structure 141 is 1000A.
[0164] In some embodiments, the first protection structure 211 includes a first end close to the compound semiconductor composite layer and a second end away from the compound semiconductor composite layer, and the second end extends to be flush with the side of the cap structure 141 away from the substrate 11. That is, the first protection structure 211 completely covers the side wall of the cap structure 141 facing the source structure 181 and / or the drain structure 182 to better protect the side wall of the cap structure 141. In other embodiments, the second end of the first protection structure 211 may not extend to be flush with the side of the cap structure 141 away from the substrate 11, that is, the second end of the first protection structure 211 may also be located on the side wall of the cap structure 141, as long as the side wall of the cap structure 141 can be protected.
[0165] In some embodiments, the width of the first protective structure 211 at the first end close to the compound semiconductor composite layer is greater than the width of the second end away from the compound semiconductor composite layer, wherein the width direction is the arrangement direction of the source structure 181 and the drain structure 182 , and this feature is formed by a dry etching process during the preparation of the first protective structure 211 .
[0166] Further, in some embodiments, the first protection structure 211 includes a side surface facing the source structure 181 and / or the drain structure 182, and the side surface is a curved surface. It can be understood that the side surface of the first protection structure 211 facing the source structure 181 and / or the drain structure 182 is a curved surface, which is also formed by the dry etching process in the process of preparing the first protection structure 211.
[0167] In some embodiments, the GaN-HEMT device further includes a first dielectric layer 17, which is disposed on the compound semiconductor composite layer and is located between the source structure 181 and the first protection structure 211, and between the first protection structure 211 and the drain structure 182. In a specific embodiment, the first dielectric layer 17 covers the surface of the barrier layer 13 of the compound semiconductor composite layer away from the channel layer 12 and the first protection structure 211, and exposes the cap structure 141. A source opening 171 and a drain opening 172 are formed in the first dielectric layer 17, and the source structure 181 and the drain structure 182 are electrically connected to the barrier layer 13 of the compound semiconductor composite layer through the source opening 171 and the drain opening 172, respectively.
[0168] In some embodiments, the GaN-HEMT device further includes a second dielectric layer 19, which covers the source structure 181, the drain structure 182, and the first dielectric layer 17 and exposes the cap structure 141. Specifically, the second dielectric layer 19 has a gate opening 191, and the gate opening 191 exposes the gate opening 191. The gate metal 20 partially covers the second dielectric layer 19, and is partially located in the gate opening 191 and electrically connected to the cap structure 141 to form a gate structure.
[0169] It can be understood that by providing a first protective structure 211 extending along the side wall from the surface of the compound semiconductor composite layer toward a direction away from the substrate 11 on the side wall of the cap structure 141, the first protective structure 211 protects the side of the cap structure 141, which can effectively reduce damage to the cap structure 141, reduce the risk of gate leakage, and improve the gate control capability and device reliability.
[0170] See also Fig. 22 In one embodiment, the second dielectric layer 19 is a flat layer, and the second dielectric layer 19 is formed by chemical mechanical polishing. The surface of the second dielectric layer 19 is flat, and does not require overexposure and development, i.e., overetching, which can avoid the problem of dielectric sidewall thinning caused by dielectric deposition height difference, effectively reduce gate leakage, improve gate control capability, and improve device reliability. In another embodiment, Fig.23 As shown, the second dielectric layer 19 may also be a non-planar layer, that is, the second dielectric layer 19 may not be planarized by using a chemical mechanical polishing process.
[0171] In some embodiments, the material of the first protection structure 211 is Si x Oy, wherein x>0 and y>0, preferably, x:y≥1:2, for example, the material of the first protection structure 211 may be SiO2 or Si2O3, or may be other amorphous silicon oxides. x Oy The material can be a silicon-rich material. The silicon-rich oxide material can enhance the network structure of the material and has higher hardness and wear resistance. It can improve the wear resistance or scratch resistance and enhance the mechanical properties of the first protective structure 211 to better protect the cap structure 141.
[0172] The specific structure of GaN-HEMT devices can be referred to Fig. 22 or Fig.23 The specific structure and function of any of the GaN-HEMT devices shown are described in the above-mentioned method for preparing the GaN-HEMT device, and will not be repeated here.
[0173] The cap structure 141 of the GaN-HEMT device provided in the present application has less surface damage, a lower risk of gate leakage, a stronger gate control capability, and a higher device reliability.
[0174] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A GaN-HEMT device, characterized in that: include: substrate; A compound semiconductor composite layer generating a two-dimensional electron gas is arranged on the substrate; An electrode structure, comprising: a source structure, a gate structure and a drain structure, arranged on the compound semiconductor composite layer, wherein the gate structure is located between the source structure and the drain structure; The gate structure comprises: a cap structure disposed on the compound semiconductor composite layer and a gate metal disposed on the cap structure; The cap structure comprises: a side wall facing the source structure and / or the drain structure; The first protection structure extends from the surface of the compound semiconductor composite layer along the side wall in a direction away from the substrate, and the first protection structure is located between the side wall and its corresponding electrode structure.
2. The GaN-HEMT device according to claim 1, characterized in that: The first protection structure includes: a first end close to the compound semiconductor composite layer, and a second end away from the compound semiconductor composite layer, wherein the second end extends to be flush with a side of the cap structure away from the substrate.
3. The GaN-HEMT device according to claim 2, characterized in that: The width of the first end is greater than the width of the second end, and the width direction is the arrangement direction of the source structure and the drain structure.
4. The GaN-HEMT device according to claim 3, characterized in that: The first protection structure includes a side surface facing the source structure and / or the drain structure, and the side surface is a curved surface.
5. The GaN-HEMT device according to claim 2, characterized in that: The GaN-HEMT device further comprises: The first dielectric layer is disposed on the compound semiconductor composite layer and is located between the source structure and the first protection structure, and between the first protection structure and the drain structure.
6. The GaN-HEMT device according to claim 5, characterized in that: The GaN-HEMT device further comprises: The second dielectric layer is disposed on the first dielectric layer, and the second dielectric layer is a planarization layer.
7. The GaN-HEMT device according to claim 1, characterized in that: The material of the first protection structure is Si x O y , x>0 and y>0.
8. A method for preparing a GaN-HEMT device, characterized in that: include: A preform of a GaN-HEMT device is provided; the preform of the GaN-HEMT device comprises a stacked substrate and a compound semiconductor composite layer generating a two-dimensional electron gas, a cap structure, a second protection structure, a first dielectric layer, a source-drain electrode layer, a second dielectric layer, and a first protection structure; wherein the source-drain electrode layer comprises a source electrode structure and a drain electrode structure arranged at intervals; the cap structure is located between the source electrode structure and the drain electrode structure, and comprises a side wall facing the source electrode structure and / or the drain electrode structure, and the first protection structure is arranged on the side wall; the second protection structure covers the top wall of the cap structure, and the first dielectric layer covers the first protection structure, the second protection structure and the compound semiconductor composite layer; the second dielectric layer covers the source electrode structure, the drain structure and the first dielectric layer; Processing the second dielectric layer and the first dielectric layer to expose the second protective structure; etching and removing the second protection structure by a wet etching process to expose the cap structure; A gate metal is formed on a side of the second dielectric layer away from the first dielectric layer; the gate metal is electrically connected to the cap structure to serve as a gate structure.
9. The method for preparing a GaN-HEMT device according to claim 8, characterized in that: The step of providing a preform of a GaN-HEMT device comprises: Providing a GaN substrate; the GaN substrate comprises the substrate, the compound semiconductor composite layer and the cap layer which are stacked in sequence; forming a second protective layer on a side of the cap layer away from the compound semiconductor composite layer; the second protective layer covers the cap layer; Patterning the second protection layer and the capping layer to form the second protection structure and the capping structure which are stacked; forming a first protective layer on a side of the second protective structure away from the compound semiconductor composite layer; the first protective layer covers the second protective structure and the compound semiconductor composite layer; patterning the first protection layer to form the first protection structure; forming the first dielectric layer on a side of the second protection structure away from the compound semiconductor composite layer; The source-drain electrode layer is formed on a side of the first dielectric layer away from the compound semiconductor composite layer; wherein the thickness of the second protective layer is greater than the thickness of the source-drain electrode layer; The second dielectric layer is formed on a side of the source and drain electrode layer away from the compound semiconductor composite layer.
10. The method for preparing a GaN-HEMT device according to claim 9, characterized in that: The step of forming a second protective layer on a side of the cap layer away from the compound semiconductor composite layer comprises: Si is deposited on the entire surface of the cap layer away from the compound semiconductor composite layer. x O y Layer; wherein x>0 and y>0; The step of forming a first protective layer on a side of the second protective structure away from the compound semiconductor composite layer specifically includes: Si is deposited on the entire surface of the second protection structure away from the compound semiconductor composite layer and the surface of the compound semiconductor composite layer away from the substrate. x O y Layer; wherein x>0 and y>0.
11. The method for preparing a GaN-HEMT device according to claim 9, characterized in that: The step of patterning the second protective layer and the capping layer specifically includes: forming a second photoresist layer on a side of the second protective layer away from the cap layer; patterning the second photoresist layer using a mask to form a second photoresist pattern; Removing the portion of the second protection layer and the portion of the capping layer not covered by the second photoresist pattern by dry etching; The step of patterning the first protective layer to form the first protective structure specifically includes: forming a first photoresist layer on a side of the first protective layer away from the compound semiconductor composite layer; Patterning the first photoresist layer using a mask to form a first photoresist pattern; The portion of the first protection layer not covered by the first photoresist pattern is removed by etching using a dry etching process.
12. The method for preparing a GaN-HEMT device according to claim 9, characterized in that: The step of forming the first dielectric layer on the side of the second protection structure away from the compound semiconductor composite layer and the step of forming the second dielectric layer on the side of the source and drain layer away from the compound semiconductor composite layer both include depositing Si a N b Layer, where a>0 and b>0.
13. The method for preparing a GaN-HEMT device according to claim 9, characterized in that: The step of forming the source-drain electrode layer on a side of the first dielectric layer away from the compound semiconductor composite layer comprises: forming a source opening and a drain opening on the first dielectric layer; Depositing a first metal layer on a surface of the first dielectric layer away from the compound semiconductor composite layer; The first metal layer is patterned.
14. The method for preparing a GaN-HEMT device according to any one of claims 8 to 13, characterized in that: The step of processing the second dielectric layer and the first dielectric layer to expose the second protective structure includes: The second dielectric layer is planarized by using a chemical mechanical polishing process to remove the portion of the first dielectric layer covering the second protective structure and make the surface of the second dielectric layer away from the substrate into a plane, thereby exposing the second protective structure; Alternatively, the second dielectric layer and the first dielectric layer are etched by a dry etching process to expose the second protection structure.
15. The method for preparing a GaN-HEMT device according to claim 14, characterized in that: The step of etching the second dielectric layer and the first dielectric layer by a dry etching process to expose the second protection structure includes: The second dielectric layer and the first dielectric layer are etched using inductively coupled plasma.
16. The method for preparing a GaN-HEMT device according to any one of claims 8 to 13, characterized in that: The step of removing the second protection structure by a wet etching process to expose the cap structure comprises: The second protection structure is etched using a buffered oxide etchant; the etching rate of the buffered oxide etchant on the second protection structure is greater than the etching rate on the second dielectric layer and the first dielectric layer.
17. The method for preparing a GaN-HEMT device according to claim 16, characterized in that: The materials of the second dielectric layer and the first dielectric layer are both Si a N b The material of the second protection structure and the first protection structure is Si x O y ; Where a>0 and b>0, x>0 and y>0; The buffered oxide etchant comprises NH4F and HF, wherein the volume ratio of the NH4F to the HF is 3:1-8:1; the buffered oxide etchant etches Si x O y The rate is 1500A / min-2000A / min, and the buffered oxide etching solution etches Si a N b The rate is 400A / min-600A / min.
Citation Information
Cited By
Semiconductor device and preparation method thereof, chip and electronic equipment
CN119208266A