Solid-state sodium metal battery and preparation method thereof

By forming an interface improvement layer for conducting sodium ions in a solid sodium battery, the interface problem between the sodium metal negative electrode and the solid electrolyte of the sodium-based fast ion conductor is solved, and the circulation performance and stability of the battery are improved.

CN118763291BActive Publication Date: 2024-11-26SHENZHEN HANKE NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411208493.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-26
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

There are high impedance and uneven deposition of sodium ions in solid sodium batteries, resulting in reduced cell circulation performance.

Method used

The first interface improvement layer and the second interface improvement layer are formed between the sodium-based solid electrolyte layer and the negative electrode sheet, and the inorganic intermediate layer and metal intermediate layer are formed on the surface of the sodium-based solid electrolyte layer, and heat treatment is performed under a protective atmosphere , the metal intermediate layer and the inorganic intermediate layer undergo a replacement reaction to generate sodium-based inorganic substances that conduct sodium ions; at the same time, the negative electrode sheet is surface treated to make it come into contact with the reaction gas to generate sodium-based inorganic substances that conduct sodium ions .

Benefits of technology

Reduces the interface impedance between the sodium-based solid electrolyte layer and the negative electrode sheet, promotes the uniform deposition of sodium on the surface of the negative electrode sheet, improves the interface stability, improves the sodium ion field distribution and dendrite growth problems, and improves the circulation of the battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763291B_ABST
    Figure CN118763291B_ABST
Patent Text Reader

Abstract

The present invention relates to a solid-state sodium metal battery and a method for preparing the same. The solid-state sodium metal battery and the method for preparing the same form a first interface improvement layer on a sodium-based solid electrolyte layer by a first surface treatment; and / or, form a second interface improvement layer on a negative electrode plate by a second surface treatment. The first surface treatment step includes: forming an inorganic intermediate layer on the surface of the sodium-based solid electrolyte layer, and forming a metal intermediate layer on the inorganic intermediate layer; performing heat treatment under a protective atmosphere to melt the metal intermediate layer and react with the inorganic intermediate layer to obtain the first interface improvement layer. The second surface treatment step includes: heating the negative electrode plate under a protective atmosphere, and contacting the negative electrode plate with a reaction gas to react to obtain the second interface improvement layer. The above-mentioned interface improvement layer can reduce the interface impedance between the sodium-based solid electrolyte layer and the negative electrode plate, especially the sodium metal negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical energy storage, and in particular to a solid-state sodium metal battery and a preparation method thereof. Background Art

[0002] The theoretical capacity of the sodium metal negative electrode reaches 1165mAh / g, and the potential relative to the standard hydrogen electrode is -2.71V. In addition, sodium metal reserves are abundant and the cost is low. It has great application potential in energy storage grids, power batteries and other fields. Liquid sodium ion batteries have problems such as volatile and flammable electrolytes. Therefore, using sodium-based solid electrolytes to replace electrolytes can improve the safety performance of sodium batteries.

[0003] However, since both the electrodes and electrolytes of solid-state batteries are solid, there is a solid-solid point contact between the electrodes and the solid electrolyte, which often leads to poor carrier transport at the interface. The interface problem between the sodium metal negative electrode and the sodium fast ion conductor solid electrolyte in solid-state sodium batteries often leads to high impedance at the interface and uneven deposition of sodium ions, which in turn leads to the growth of sodium dendrites along the grain boundaries and pores of the solid electrolyte. Eventually, the dendrites penetrate the solid electrolyte, causing a short circuit in the battery and reducing the battery cycle performance. Summary of the invention

[0004] Based on this, it is necessary to provide a solid-state sodium metal battery and a preparation method thereof to improve the interface problem between the electrode and the solid electrolyte.

[0005] A method for preparing a solid-state sodium metal battery comprises the following steps:

[0006] Providing a positive electrode plate, a sodium-based solid electrolyte layer and a negative electrode plate, wherein the material of the negative electrode plate includes metallic sodium;

[0007] Performing a first surface treatment on a side of the sodium-based solid electrolyte layer facing the negative electrode plate to form a first interface improvement layer on the sodium-based solid electrolyte layer; and / or performing a second surface treatment on a side of the negative electrode plate facing the sodium-based solid electrolyte layer to form a second interface improvement layer on the negative electrode plate;

[0008] The positive electrode sheet, the sodium-based solid electrolyte layer and the negative electrode sheet are stacked;

[0009] Wherein, the first surface treatment step comprises:

[0010] Forming an inorganic intermediate layer on the surface of the sodium-based solid electrolyte layer, wherein the material of the inorganic intermediate layer includes one or more of PBr5, NBr3, POBr3, PI3 and NI3;

[0011] forming a metal intermediate layer on the inorganic intermediate layer, wherein the material of the metal intermediate layer includes metallic sodium;

[0012] Performing heat treatment under a protective atmosphere to melt the metal intermediate layer and react with the inorganic intermediate layer to obtain the first interface improvement layer;

[0013] Wherein, the second surface treatment step comprises:

[0014] The negative electrode plate is heated under a protective atmosphere, and is contacted with a reaction gas for reaction, wherein the reaction gas includes one or more of PF3, PF5, NF3, NOF, NO2F, OF2, O2F2, O4F2 and O5F2 to obtain the second interface improvement layer.

[0015] In one embodiment, the thickness of the inorganic intermediate layer is 10 nm to 50 nm;

[0016] In one embodiment, the thickness of the metal intermediate layer is 100nm~400nm.

[0017] In one embodiment, the heat treatment temperature is 100°C to 120°C, and the time is 10min to 60min.

[0018] In one embodiment, in the step of forming the second interface improvement layer, the heating temperature of the negative electrode plate is 60° C. to 80° C., and the contact reaction time between the negative electrode plate and the reaction gas is 0.5 min to 30 min.

[0019] In one embodiment, the method for preparing the solid-state sodium metal battery further comprises the following steps:

[0020] A third interface improvement layer is formed on the side of the positive electrode sheet facing the sodium-based solid electrolyte layer, and the material of the third interface improvement layer includes NaF, NaBr, Na3N, Na2O, NaLaCl4, Na 0.7 Zr 0.3 La 0.7 At least one of Cl4, Na3YCl6, Na3InCl6 and NaTaCl6.

[0021] In one embodiment, the positive electrode sheet includes a positive electrode current collector and a positive electrode layer disposed on the positive electrode current collector, the positive electrode layer includes a mixed positive electrode material and a sodium-based solid electrolyte. The third interface improvement layer is formed on the positive electrode layer.

[0022] In one embodiment, the thickness of the third interface improvement layer is 10 nm to 40 nm.

[0023] In one embodiment, the method for preparing the solid-state sodium metal battery further comprises the following steps:

[0024] A precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate, wherein the precursor solution contains a solvent, a sodium salt dispersed in the solvent, an α-diazo lactone and a catalyst, wherein the catalyst is used to catalyze the ring-opening polymerization of the α-diazo lactone.

[0025] The precursor solution is subjected to a heating treatment to react and form a buffer layer.

[0026] In one embodiment, the sodium salt is selected from one or more of NaTFSI and NaFSI.

[0027] In one embodiment, the concentration of the sodium salt is 1 mol / L~1.5 mol / L.

[0028] In one embodiment, the α-diazo lactone is one or more of a five-membered ring α-diazo lactone, a six-membered ring α-diazo lactone, a seven-membered ring α-diazo lactone, and an eight-membered ring α-diazo lactone.

[0029] In one embodiment, the volume ratio of the α-diazo lactone to the solvent is 1: (6-10).

[0030] In one embodiment, the molar ratio of the catalyst to the α-diazolactone is 1:(55-100).

[0031] A solid-state sodium metal battery is prepared by the preparation method described in any of the above embodiments.

[0032] Compared with the conventional technology, the solid-state sodium metal battery and its preparation method have the following beneficial effects:

[0033] The solid-state sodium metal battery and its preparation method form a first interface improvement layer on the sodium-based solid electrolyte layer; and / or, form a second interface improvement layer on the negative electrode plate. By forming an inorganic intermediate layer and a metal intermediate layer of the above-mentioned material on the surface of the sodium-based solid electrolyte layer, and performing heat treatment under a protective atmosphere, the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting to generate a sodium-based inorganic substance that conducts sodium ions, and form a first interface improvement layer between the sodium-based solid electrolyte layer and the negative electrode plate. The first interface improvement layer can reduce the interface impedance between the sodium-based solid electrolyte layer and the negative electrode plate, especially the sodium metal negative electrode, and reduce the nucleation and growth barriers of sodium deposition, promote the uniform deposition of sodium on the surface of the negative electrode plate, and improve the interface stability on the negative electrode side.

[0034] By performing the above-mentioned second surface treatment on the negative electrode plate including metallic sodium, a sodium-based inorganic substance that conducts sodium ions is generated on the side of the negative electrode plate facing the sodium-based solid electrolyte layer, and a second interface improvement layer is formed between the sodium-based solid electrolyte layer and the negative electrode plate. The second interface improvement layer can improve the problems of large interface impedance between the sodium-based solid electrolyte layer and the sodium metal negative electrode plate, uneven sodium ion field distribution, and longitudinal growth of sodium dendrites. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the structure of a solid-state sodium metal battery according to an embodiment.

[0036] Description of reference numerals:

[0037] 100. solid-state sodium metal battery; 110. positive electrode plate; 120. sodium-based solid electrolyte layer; 130. negative electrode plate; 140. first interface improvement layer; 150. second interface improvement layer; 160. third interface improvement layer; 170. buffer layer. DETAILED DESCRIPTION

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0039] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0040] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0041] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0042] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0043] A method for preparing a solid-state sodium metal battery 100 according to an embodiment of the present invention comprises the following steps:

[0044] like Figure 1 As shown, a positive electrode sheet 110, a sodium-based solid electrolyte layer 120 and a negative electrode sheet 130 are provided, and the material of the negative electrode sheet 130 includes metallic sodium.

[0045] A first surface treatment is performed on the side of the sodium-based solid electrolyte layer 120 facing the negative electrode plate 130 to form a first interface improvement layer 140 on the sodium-based solid electrolyte layer 120; and / or, a second surface treatment is performed on the side of the negative electrode plate 130 facing the sodium-based solid electrolyte layer 120 to form a second interface improvement layer 150 on the negative electrode plate 130.

[0046] The positive electrode sheet 110 , the sodium-based solid electrolyte layer 120 , and the negative electrode sheet 130 are stacked.

[0047] The first surface treatment step includes:

[0048] An inorganic intermediate layer is formed on the surface of the sodium-based solid electrolyte layer 120, and the material of the inorganic intermediate layer includes one or more of PBr5 (phosphorus pentabromide), NBr3 (nitrogen tribromide), POBr3 (phosphorus oxybromide), PI3 (phosphorus triiodide), and NI3 (nitrogen triiodide);

[0049] forming a metal intermediate layer on the inorganic intermediate layer, wherein the material of the metal intermediate layer includes metallic sodium;

[0050] A heat treatment is performed under a protective atmosphere to melt the metal intermediate layer and react with the inorganic intermediate layer to obtain a first interface improvement layer.

[0051] By forming an inorganic intermediate layer and a metal intermediate layer of the above-mentioned material on the surface of the sodium-based solid electrolyte layer 120, and performing heat treatment under a protective atmosphere, the metal intermediate layer can undergo a substitution reaction with the inorganic intermediate layer after melting to generate a sodium-based inorganic substance that conducts sodium ions, and form a first interface improvement layer 140 between the sodium-based solid electrolyte layer 120 and the negative electrode plate 130. The first interface improvement layer 140 can reduce the interface impedance between the sodium-based solid electrolyte layer 120 and the negative electrode plate 130, especially the sodium metal negative electrode, and reduce the nucleation and growth barriers of sodium deposition, promote the uniform deposition of sodium on the surface of the negative electrode plate 130, and improve the interface stability on the negative electrode side.

[0052] Wherein, the second surface treatment step comprises:

[0053] The negative electrode plate 130 is heated under a protective atmosphere, and is contacted with a reaction gas to react. The reaction gas includes one or more of PF3 (phosphorus trifluoride), PF5 (phosphorus pentafluoride), NF3 (nitrogen trifluoride), NOF (nitrosyl fluoride), NO2F (nitrosyl fluoride), OF2 (oxygen difluoride), O2F2 (dioxygen difluoride), O4F2 (tetraoxygen difluoride), and O5F2 (pentaoxygen difluoride) to obtain a second interface improvement layer 150.

[0054] By performing the above-mentioned second surface treatment on the negative electrode plate 130 including metallic sodium, a sodium-based inorganic substance that conducts sodium ions is generated on the side of the negative electrode plate 130 facing the sodium-based solid electrolyte layer 120, and a second interface improvement layer 150 is formed between the sodium-based solid electrolyte layer 120 and the negative electrode plate 130. The second interface improvement layer 150 can improve the problems of large interface impedance between the sodium-based solid electrolyte layer 120 and the negative electrode plate 130 of sodium metal, uneven sodium ion field distribution, and longitudinal growth of sodium dendrites.

[0055] In some of the examples, the preparation method of the solid-state sodium metal battery 100 may perform a first surface treatment and a second surface treatment to form the above-mentioned first interface improvement layer 140 and the above-mentioned second interface improvement layer 150. For example, the surface of the sodium-based solid electrolyte layer 120 is subjected to a first surface treatment, PBr5 is deposited on the surface of the sodium-based solid electrolyte layer 120 to form an inorganic intermediate layer, metallic sodium is deposited on the inorganic intermediate layer to form a metal intermediate layer, and a heat treatment is performed to melt the metal intermediate layer and react with the inorganic intermediate layer to obtain the first interface improvement layer 140; and the surface of the negative electrode plate 130 is subjected to a second surface treatment, the negative electrode plate 130 is heated under a protective atmosphere, PF3 is introduced, and the negative electrode plate 130 is contacted with the reaction gas to react to obtain the second interface improvement layer 150. Through the cooperation of the first interface improvement layer 140 and the second interface improvement layer 150, improvements are made in many aspects, which can better improve the interface stability and improve the problems of large interface impedance.

[0056] In the first surface treatment, the material of the inorganic intermediate layer includes one or more of PBr5, NBr3, POBr3, PI3 and NI3. The above-mentioned inorganic materials react in situ with metallic sodium at the interface to generate a SEI (solid electrolyte interphase interface) membrane composed of two or three sodium-conducting compounds. The various sodium-conducting compound components have excellent electronic insulation and ion conductivity, and the synergistic effect of multiple components improves the interface stability. Compared with a single-component inorganic SEI membrane or an ion-electron mixed membrane (inorganic component plus conductive alloy) formed by a replacement reaction, a multi-component inorganic SEI membrane can better ensure the transport of sodium ions at the interface, while avoiding the reduction of the solid electrolyte by the negative electrode.

[0057] In the first surface treatment, the preparation process of the inorganic intermediate layer may be, but is not limited to, a physical vapor deposition (PVD) process, such as magnetron sputtering, evaporation, and the like.

[0058] In some of these examples, in the first surface treatment, the inorganic intermediate layer is prepared by radio frequency (RF) magnetron sputtering. During the coating, the deposition chamber is evacuated to 4×10 -5 Pa~8×10 -5 Pa, an inert gas (such as argon) with a flow rate of 60sccm~100sccm is introduced, the working pressure is controlled to be 0.2Pa~0.5Pa, and the working power is 50W~80W. In this way, a dense inorganic intermediate layer can be obtained with strong interlayer force and controllable thickness.

[0059] The vacuum degree of the deposition chamber is, for example, 4×10 -5 Pa, 4.5×10 -5 Pa, 5×10 -5 Pa, 5.5×10 -5 Pa, 6×10 -5 Pa, 6.5×10 -5 Pa, 7×10 -5 Pa, 7.5×10 -5 Pa, 8×10 -5 The flow rate of the inert gas is, for example, 60 sccm, 65 sccm, 70 sccm, 75 sccm, 80 sccm, 85 sccm, 90 sccm, 95 sccm, 100 sccm, etc. The working gas pressure is, for example, 0.2 Pa, 0.25 Pa, 0.3 Pa, 0.35 Pa, 0.4 Pa, 0.45 Pa, 0.5 Pa, etc. The working power is, for example, 50 W, 55 W, 60 W, 65 W, 70 W, 75 W, 80 W, etc.

[0060] In some of these examples, in the first surface treatment, the thickness of the inorganic intermediate layer is 10nm to 50nm. Further, in some of these examples, the thickness of the inorganic intermediate layer is 15nm to 45nm. Further, in some of these examples, the thickness of the inorganic intermediate layer is 20nm to 40nm. In some specific examples, the thickness of the inorganic intermediate layer is, for example, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, etc.

[0061] In the first surface treatment, the preparation process of the metal intermediate layer may be, but is not limited to, a physical vapor deposition (PVD) process, such as magnetron sputtering, evaporation, and the like.

[0062] In some of these examples, in the first surface treatment, the metal intermediate layer is prepared by a direct current (DC) magnetron sputtering process. During the coating, the deposition chamber is evacuated to 4×10 -5 Pa~8×10 -5 Pa, an inert gas (such as argon) with a flow rate of 60sccm~100sccm is introduced, the working pressure is controlled to be 0.2Pa~0.5Pa, and the working power is 50W~100W. In this way, a dense metal intermediate layer can be obtained with strong interlayer strength and controllable thickness.

[0063] The vacuum degree of the deposition chamber is, for example, 4×10 -5 Pa, 4.5×10 -5 Pa, 5×10 -5 Pa, 5.5×10 - 5 Pa, 6×10 -5 Pa, 6.5×10 -5 Pa, 7×10 -5 Pa, 7.5×10 -5Pa, 8×10 -5 The flow rate of the inert gas is, for example, 60 sccm, 65 sccm, 70 sccm, 75 sccm, 80 sccm, 85 sccm, 90 sccm, 95 sccm, 100 sccm, etc. The working gas pressure is, for example, 0.2 Pa, 0.25 Pa, 0.3 Pa, 0.35 Pa, 0.4 Pa, 0.45 Pa, 0.5 Pa, etc. The working power is, for example, 50 W, 55 W, 60 W, 65 W, 70 W, 75 W, 80 W, 85 W, 90 W, 95 W, 100 W, etc.

[0064] In some of these examples, in the first surface treatment, the thickness of the metal intermediate layer is 100nm~400nm. Further, in some of these examples, the thickness of the metal intermediate layer is 150nm~350nm. Further, in some of these examples, the thickness of the metal intermediate layer is 200nm~300nm. In some specific examples, the thickness of the metal intermediate layer is 100nm, 130nm, 160nm, 190nm, 220nm, 250nm, 280nm, 310nm, 330nm, 360nm, 390nm, 400nm, etc.

[0065] In some of the examples, in the first surface treatment, the temperature of the heat treatment is 100°C to 120°C. Further, in some of the examples, the temperature of the heat treatment is 105°C to 115°C. Further, in some of the examples, the temperature of the heat treatment is 108°C to 112°C. In some specific examples, the temperature of the heat treatment is, for example, 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C, 120°C, etc.

[0066] Optionally, in the first surface treatment, the protective atmosphere may be, but is not limited to, argon.

[0067] In some of these examples, in the first surface treatment, the time of the heat treatment is 10min to 60min. Further, in some of these examples, the time of the heat treatment is 20min to 50min. Further, in some of these examples, the time of the heat treatment is 30min to 40min. In some specific examples, the time of the heat treatment is, for example, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, 60min, etc.

[0068] In one example, in the second surface treatment, the heating temperature of the negative electrode plate 130 is 60°C to 80°C. Further, in some of the examples, the heating temperature of the negative electrode plate 130 is 65°C to 75°C. Further, in some of the examples, the heating temperature of the negative electrode plate 130 is 68°C to 72°C. In some specific examples, the heating temperature of the negative electrode plate 130 is, for example, 60°C, 62°C, 64°C, 66°C, 68°C, 70°C, 72°C, 74°C, 76°C, 78°C, 80°C, etc.

[0069] In some of the examples, in the second surface treatment, the time for the negative electrode plate 130 to contact and react with the reaction gas is 0.5 min to 30 min. Further, in some of the examples, the time for the negative electrode plate 130 to contact and react with the reaction gas is 2 min to 25 min. Further, in some of the examples, the time for the negative electrode plate 130 to contact and react with the reaction gas is 5 min to 20 min. In some specific examples, the time for the negative electrode plate 130 to contact and react with the reaction gas is, for example, 0.5 min, 1 min, 3 min, 6 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.

[0070] Optionally, in the second surface treatment, the protective atmosphere may be, but is not limited to, argon.

[0071] In one example, the method for preparing the solid-state sodium metal battery 100 further includes the following steps:

[0072] A third interface improvement layer 160 is formed on the side of the positive electrode sheet 110 facing the sodium-based solid electrolyte layer 120. The material of the third interface improvement layer 160 includes NaF, NaBr, Na3N, Na2O, NaLaCl4, Na 0.7 Zr 0.3 La 0.7 At least one of Cl4, Na3YCl6, Na3InCl6 and NaTaCl6.

[0073] In order to solve the problem that the de-sodium positive electrode may oxidize the polymer, a third interface improvement layer 160 of the above material is formed between the positive electrode plate 110 and the sodium-based solid electrolyte layer 120 to prevent the electrode active material from oxidizing the electrolyte material and improve the interface conductivity. The third interface improvement layer 160 can protect the polymer and improve ion conduction.

[0074] Furthermore, the material of the third interface improvement layer 160 includes NaLaCl4, Na 0.7 Zr 0.3 La 0.7At least one of Cl4, Na3YCl6, Na3InCl6, and NaTaCl6. The above materials are all halide sodium fast ion conductors with better sodium ion conductivity. Coating the surface of the positive electrode material can reduce the transmission impedance of sodium ions at the positive electrode interface.

[0075] In some examples, the positive electrode sheet 110 includes a positive electrode current collector and a positive electrode layer. The positive electrode layer is disposed on the positive electrode current collector. The third interface improvement layer 160 is formed on the positive electrode layer.

[0076] Illustratively, the positive electrode current collector includes, for example, aluminum foil.

[0077] In some of the examples, the positive electrode layer comprises a mixed positive electrode material and a sodium-based solid electrolyte. Further, in some of the examples, the weight portion of the positive electrode material is 45-55 parts, and the weight portion of the sodium-based solid electrolyte is 25-35 parts. Further, in some of the examples, the weight portion of the positive electrode material is 47-53 parts, and the weight portion of the sodium-based solid electrolyte is 27-33 parts. Further, in some of the examples, the weight portion of the positive electrode material is 50 parts, and the weight portion of the sodium-based solid electrolyte is 30 parts.

[0078] In some examples, the cathode materials include Na3V2(PO4)3, Na2MnP2O7, NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 At least one of O2, Na2CoFe(CN)6.

[0079] In some examples, the sodium-based solid electrolyte includes at least one of a sodium superionic conductor electrolyte and a borohydride. For example, the sodium superionic conductor electrolyte may be, but is not limited to, Na3Zr2Si2PO 12 、Na 3.2 Zr 1.9 Ca 0.1 Si2PO 12 、Na 3.2 Zr 1.9 Mg 0.1 Si2PO 12 For example, the borohydride may be, but is not limited to, Na4B 36 H 34 -7Na2B 12 H 12 , Na2B 10 H 10 -Na2B 12 H 12 At least one of .

[0080] The sodium-based solid electrolyte layer 120 and the sodium-based solid electrolyte may be the same or different.

[0081] It can be understood that the positive electrode layer may further include a binder, a conductive agent, etc. The weight percentage of the positive electrode binder is, for example, 8 to 12 parts, and further, the weight percentage of the positive electrode binder is, for example, 9 to 11 parts. The weight percentage of the positive electrode conductive agent is, for example, 8 to 12 parts, and further, the weight percentage of the positive electrode conductive agent is, for example, 9 to 11 parts.

[0082] Illustratively, the binder of the positive electrode includes one or more of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, epoxy resin and nylon.

[0083] Illustratively, the conductive agent of the positive electrode includes one or more of carbon black, acetylene black and Ketjen black.

[0084] In one example, the thickness of the third interface improvement layer 160 is 10nm~40nm. Further, in some of these examples, the thickness of the inorganic intermediate layer is 15nm~35nm. Further, in some of these examples, the thickness of the third interface improvement layer 160 is 20nm~30nm. In some specific examples, the thickness of the third interface improvement layer 160 is, for example, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, etc.

[0085] In one example, the method for preparing the solid-state sodium metal battery 100 further includes the following steps:

[0086] A precursor solution is added between the sodium-based solid electrolyte layer 120 and the positive electrode plate 110 . The precursor solution contains a solvent, a sodium salt dispersed in the solvent, α-diazolactone, and a catalyst. The catalyst is used to catalyze the ring-opening polymerization of α-diazolactone.

[0087] The heat treatment is performed to react the precursor solution to form the buffer layer 170 .

[0088] In the above example, a polymer-based buffer layer 170 formed by in-situ polymerization is introduced between the positive electrode plate 110 and the sodium-based solid electrolyte layer 120. The buffer layer 170 has good flexibility and can improve the interface contact problem. The above precursor solution is also added with sodium salt, which can disperse Na ions in the polymer electrolyte by dissociation, and promote the migration of sodium ions as the polymer chain segments swing. The diazo-group polyester polymer obtained by the polymerization of α-diazo lactone has excellent oxidative stability under high voltage, can match the high-voltage positive electrode, release more capacity under high voltage, and improve the energy density of the battery.

[0089] Optionally, the sodium salt may be, but is not limited to, one or more of NaTFSI (sodium bis(trifluoromethanesulfonyl)imide) and NaFSI (sodium bis(fluorosulfonyl)imide). NaTFSI and NaFSI sodium salts have good solubility and high ion conductivity, and will not produce Lewis acid to affect the stability of THF solvent.

[0090] In one example, the concentration of sodium salt is 1 mol / L to 1.5 mol / L, for example, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, etc.

[0091] In one example, the α-diazo lactone is one or more of a five-membered ring α-diazo lactone, a six-membered ring α-diazo lactone, a seven-membered ring α-diazo lactone, and an eight-membered ring α-diazo lactone.

[0092] In one example, the volume ratio of α-diazo lactone to solvent is 1: (6-10). Further, in one example, the volume ratio of α-diazo lactone to solvent is 1: (7-9). In some specific examples, the volume ratio of α-diazo lactone to solvent is 1: 6, 1: 6.5, 1: 7, 1: 7.5, 1: 8, 1: 8.5, 1: 9, 1: 9.5, 1: 10, etc.

[0093] In one example, the molar ratio of the catalyst to the α-diazo lactone is 1: (55-100). Further, in one example, the molar ratio of the catalyst to the α-diazo lactone is 1: (65-85). In some specific examples, the molar ratio of the catalyst to the α-diazo lactone is 1: 55, 1: 60, 1: 65, 1: 70, 1: 75, 1: 80, 1: 85, 1: 90, 1: 95, 1: 100, etc.

[0094] Alternatively, the solvent may be, but is not limited to, THF (tetrahydrofuran).

[0095] In one example, the temperature of the heating treatment is 60° C. to 80° C. Further, in one example, the temperature of the heating treatment is 65° C. to 75° C. In some specific examples, the temperature of the heating treatment is, for example, 60° C., 62° C., 64° C., 66° C., 68° C., 70° C., 72° C., 74° C., 76° C., 78° C., 80° C., etc.

[0096] In one example, the heating time is 2 hours to 8 hours. Further, in one example, the heating time is 3 hours to 7 hours. In some specific examples, the heating time is 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours, 6 hours, 6.5 hours, 7 hours, 7.5 hours, 8 hours, etc.

[0097] Furthermore, the present invention also provides a solid-state sodium metal battery, which is prepared by any of the preparation methods described in the above examples.

[0098] The following specific examples are provided to further illustrate the present invention. The present invention provides the following specific examples for a better understanding of the present invention, but is not limited to the specific implementation methods and does not limit the protection scope of the present invention.

[0099] Example 1

[0100] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0101] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0102] Step 1, preparation of positive electrode sheet:

[0103] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0104] Step 2, preparation of negative electrode sheet:

[0105] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0106] Step 3, interface modification of sodium-based solid electrolyte layer:

[0107] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12The sodium-based solid electrolyte layer was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 80sccm, the working gas pressure is controlled to be 0.3Pa, the working power is 50W, and PBr5 is deposited on the negative electrode side of the sodium-based solid electrolyte layer in RF mode with a thickness of 20nm to form an inorganic intermediate layer. Subsequently, a DC mode is adopted with a working power of 100W to deposit metallic sodium on the surface of the inorganic intermediate layer with a thickness of 250nm to form a metal intermediate layer. Then, heat treatment is carried out in an Ar gas atmosphere at a heat treatment temperature of 110°C for 20min, so that the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting, generating a sodium-based inorganic substance that conducts sodium ions, and forming an interface improvement layer on the sodium-based solid electrolyte layer.

[0108] Step 4, preparation of solid-state sodium metal battery:

[0109] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0110] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0111] Example 2

[0112] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0113] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0114] Step 1, preparation of positive electrode sheet:

[0115] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12, conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0116] Step 2, preparation of negative electrode sheet:

[0117] A sodium metal sheet with a thickness of 0.45 mm was taken, placed in an argon environment, heated to 60° C., and then PF3 reaction gas was introduced and reacted for 5 minutes to obtain a negative electrode sheet.

[0118] Step 3, preparation of sodium-based solid electrolyte layer:

[0119] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 , thickness is 0.4mm.

[0120] Step 4, preparation of solid-state sodium metal battery:

[0121] The sodium-based solid electrolyte layer prepared in step 3 is disposed between the sodium metal pole piece and the sodium metal pole piece prepared in step 2 to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0122] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0123] Example 3

[0124] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0125] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0126] Step 1, preparation of positive electrode sheet:

[0127] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0128] Step 2, preparation of negative electrode sheet:

[0129] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0130] Step 3, interface modification of sodium-based solid electrolyte layer:

[0131] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 The sodium-based solid electrolyte layer was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 80sccm, the working gas pressure is controlled to be 0.3Pa, the working power is 50W, and PI3 is deposited on the negative electrode side of the sodium-based solid electrolyte layer in RF mode with a thickness of 20nm to form an inorganic intermediate layer. Subsequently, a DC mode is adopted with a working power of 100W to deposit metallic sodium on the surface of the inorganic intermediate layer with a thickness of 250nm to form a metal intermediate layer. Then, heat treatment is carried out in an Ar gas atmosphere at a heat treatment temperature of 110°C for 20min, so that the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting, generating a sodium-based inorganic substance that conducts sodium ions, and forming an interface improvement layer on the sodium-based solid electrolyte layer.

[0132] Step 4, preparation of solid-state sodium metal battery:

[0133] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0134] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0135] Example 4

[0136] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0137] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0138] Step 1, preparation of positive electrode sheet:

[0139] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0140] Step 2, preparation of negative electrode sheet:

[0141] A sodium metal sheet with a thickness of 0.45 mm was taken, placed in an argon environment, heated to 60° C., and then introduced into the NF3 reaction gas for 5 minutes to obtain a negative electrode sheet.

[0142] Step 3, preparation of sodium-based solid electrolyte layer:

[0143] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 , thickness is 0.4mm.

[0144] Step 4, preparation of solid-state sodium metal battery:

[0145] The sodium-based solid electrolyte layer prepared in step 3 is disposed between the sodium metal pole piece and the sodium metal pole piece prepared in step 2 to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0146] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0147] Example 5

[0148] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0149] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0150] Step 1, preparation of positive electrode sheet:

[0151] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0152] Step 2, preparation of negative electrode sheet:

[0153] A sodium metal sheet with a thickness of 0.45 mm was taken, placed in an argon environment, heated to 60° C., and then introduced with NOF reaction gas, reacted for 5 minutes, to obtain a negative electrode sheet.

[0154] Step 3, preparation of sodium-based solid electrolyte layer:

[0155] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO12 , thickness is 0.4mm.

[0156] Step 4, preparation of solid-state sodium metal battery:

[0157] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0158] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0159] Example 6

[0160] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0161] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0162] Step 1, preparation of positive electrode sheet:

[0163] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0164] Step 2, preparation of negative electrode sheet:

[0165] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0166] Step 3, interface modification of sodium-based solid electrolyte layer:

[0167] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 The sodium-based solid electrolyte layer was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 80sccm, the working gas pressure is controlled to be 0.3Pa, the working power is 50W, and POBr3 is deposited on the negative electrode side of the sodium-based solid electrolyte layer in RF mode with a thickness of 20nm to form an inorganic intermediate layer. Subsequently, a DC mode is adopted with a working power of 100W to deposit metallic sodium on the surface of the inorganic intermediate layer with a thickness of 250nm to form a metal intermediate layer. Then, heat treatment is carried out in an Ar gas atmosphere at a heat treatment temperature of 110°C for 20min, so that the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting, generating a sodium-based inorganic substance that conducts sodium ions, and forming an interface improvement layer on the sodium-based solid electrolyte layer.

[0168] Step 4, preparation of solid-state sodium metal battery:

[0169] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0170] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0171] Example 7

[0172] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0173] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0174] Step 1, preparation of positive electrode sheet:

[0175] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12, conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0176] Step 2, preparation of negative electrode sheet:

[0177] A sodium metal sheet with a thickness of 0.45 mm was taken, placed in an argon environment, heated to 60° C., and then PF3 reaction gas was introduced and reacted for 5 minutes to obtain a negative electrode sheet.

[0178] Step 3, interface modification of sodium-based solid electrolyte layer:

[0179] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 The sodium-based solid electrolyte layer was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 80sccm, the working gas pressure is controlled to be 0.3Pa, the working power is 50W, and PBr5 is deposited on the negative electrode side of the sodium-based solid electrolyte layer in RF mode with a thickness of 20nm to form an inorganic intermediate layer. Subsequently, a DC mode is adopted with a working power of 100W to deposit metallic sodium on the surface of the inorganic intermediate layer with a thickness of 250nm to form a metal intermediate layer. Then, heat treatment is carried out in an Ar gas atmosphere at a heat treatment temperature of 110°C for 20min, so that the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting, generating a sodium-based inorganic substance that conducts sodium ions, and forming an interface improvement layer on the sodium-based solid electrolyte layer.

[0180] Step 4, preparation of solid-state sodium metal battery:

[0181] The sodium-based solid electrolyte layer prepared in step 3 is disposed between the sodium metal pole piece and the sodium metal pole piece prepared in step 2 to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0182] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0183] Example 8

[0184] This embodiment provides a solid-state sodium metal battery and a method for preparing the same.

[0185] The preparation method of the solid-state sodium metal battery of this embodiment comprises the following steps:

[0186] Step 1, preparation of positive electrode sheet:

[0187] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas was introduced, the flow rate of argon gas was 40sccm, the working pressure was controlled to be 0.3Pa, the working power was 60W, and Na was deposited on the positive electrode layer using RF mode. 0.7 Zr 0.3 La 0.7 Cl4, with a thickness of 20nm, forms a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0188] Step 2, preparation of negative electrode sheet:

[0189] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0190] Step 3, interface modification of sodium-based solid electrolyte layer:

[0191] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 The sodium-based solid electrolyte layer was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5Pa, argon gas is introduced, the flow rate of argon gas is 80sccm, the working gas pressure is controlled to be 0.3Pa, the working power is 50W, and PBr5 is deposited on the negative electrode side of the sodium-based solid electrolyte layer in RF mode with a thickness of 20nm to form an inorganic intermediate layer. Subsequently, a DC mode is adopted with a working power of 100W to deposit metallic sodium on the surface of the inorganic intermediate layer with a thickness of 250nm to form a metal intermediate layer. Then, heat treatment is carried out in an Ar gas atmosphere at a heat treatment temperature of 110°C for 20min, so that the metal intermediate layer can undergo a replacement reaction with the inorganic intermediate layer after melting, generating a sodium-based inorganic substance that conducts sodium ions, and forming an interface improvement layer on the sodium-based solid electrolyte layer.

[0192] Step 4, preparation of solid-state sodium metal battery:

[0193] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0194] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0195] Comparative Example 1

[0196] The preparation method of the solid-state sodium metal battery of this comparative example comprises the following steps:

[0197] Step 1, preparation of positive electrode sheet:

[0198] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent is added for homogenization to obtain positive electrode slurry. The positive electrode slurry is coated on the positive electrode collector (Al foil), and a positive electrode layer is formed after vacuum drying to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10 mm for standby use.

[0199] Step 2, preparation of negative electrode sheet:

[0200] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0201] Step 3, preparation of solid-state sodium metal battery:

[0202] Sodium-based solid electrolyte uses Na3Zr2Si2PO 12 , thickness is 0.4mm.

[0203] A sodium-based solid electrolyte was placed between sodium metal pole pieces to prepare a symmetrical battery, which was placed at 80°C for 4 hours for critical current density testing.

[0204] The sodium-based solid electrolyte was placed between the positive electrode sheet prepared in step 1 and the negative electrode sheet prepared in step 2, and left at 80° C. for 4 hours.

[0205] Comparative Example 2

[0206] The preparation method of the solid-state sodium metal battery of this comparative example comprises the following steps:

[0207] Step 1, preparation of positive electrode sheet:

[0208] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0209] Step 2, preparation of negative electrode sheet:

[0210] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0211] Step 3, preparation of sodium-based solid electrolyte layer:

[0212] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 , thickness is 0.4mm.

[0213] Step 4, preparation of solid-state sodium metal battery:

[0214] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0215] The sodium-based solid electrolyte layer prepared in step 3 is set between the positive electrode plate prepared in step 1 and the negative electrode plate prepared in step 2, and 40µL of the precursor solution is added between the sodium-based solid electrolyte layer and the positive electrode plate. The precursor solution is prepared in advance in the cold well (0°C) of the glove box. The preparation process is as follows: dissolve the sodium salt NaTFSI in the THF solvent, and the concentration of the sodium salt is 1mol / L. Then add the seven-membered ring α-diazo lactone, the volume ratio of the seven-membered ring α-diazo lactone to THF is 1:7, and mix evenly. Then add potassium tert-butoxide catalyst, and the molar ratio of the catalyst to is 1:70. After the battery is assembled, it is placed at room temperature for 2h, and then placed at 80°C for 4h.

[0216] Comparative Example 3

[0217] The preparation method of the solid-state sodium metal battery of this comparative example comprises the following steps:

[0218] Step 1, preparation of positive electrode sheet:

[0219] Weigh Na3V2(PO4)3, Na3Zr2Si2PO 12 , conductive agent SP and binder PVDF, with a mass ratio of 50:30:10:10, and NMP solvent was added for homogenization to obtain a positive electrode slurry. The positive electrode slurry was coated on the positive electrode current collector (Al foil) and vacuum dried to form a positive electrode layer. The positive electrode slurry was transferred to the deposition chamber of the magnetron sputtering equipment and the deposition chamber was evacuated to 6×10 -5 Pa, argon gas is introduced, the flow rate of argon gas is 40sccm, the working pressure is controlled to be 0.2Pa, the working power is 50W, and NaF is deposited on the positive electrode layer in RF mode with a thickness of 20nm to form a surface improvement layer to prepare a positive electrode sheet. The positive electrode sheet is punched to obtain a round sheet with a diameter of 10mm for standby use.

[0220] Step 2, preparation of negative electrode sheet:

[0221] The negative electrode plate uses a sodium metal sheet with a thickness of 0.45 mm, which is made into a disc with a diameter of 14 mm for standby use.

[0222] Step 3, preparation of sodium-based solid electrolyte layer:

[0223] The sodium-based solid electrolyte layer uses Na3Zr2Si2PO 12 , thickness is 0.4mm.

[0224] Step 4, preparation of solid-state sodium metal battery:

[0225] The sodium-based solid electrolyte layer prepared in step 3 is set between the sodium metal pole pieces and the sodium metal pole pieces to prepare a symmetrical battery, which is placed at 80° C. for 4 hours for critical current density testing.

[0226] The sodium-based solid electrolyte was placed between the positive electrode sheet prepared in step 1 and the negative electrode sheet prepared in step 2, and left at 80° C. for 4 hours.

[0227] The solid-state sodium metal battery prepared in the above examples and comparative examples was subjected to a charge and discharge cycle performance test under 0.5C / 0.5C conditions, and the number of cycles when the battery capacity decayed to 80% of the initial capacity was recorded. The performance test results are shown in Table 1.

[0228] Table 1 Performance test results of solid-state sodium metal batteries

[0229]

[0230] It can be seen from the test results in Table 1 that compared with Comparative Examples 1 to 3, the critical current density of the symmetrical batteries prepared in Examples 1 to 8 is significantly improved. The critical current density reflects the electrochemical stability between the sodium metal negative electrode and the sodium-based solid electrolyte layer. The higher the critical current density, the better the electrochemical stability between the sodium metal negative electrode and the solid electrolyte. In addition, compared with Comparative Examples 1 to 3, the cycle performance of the solid-state sodium metal battery prepared in Examples 1 to 8 is significantly improved, which is due to the improvement of the interface between the electrode and the sodium-based solid electrolyte layer.

[0231] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0232] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A method for preparing a solid-state sodium metal battery, characterized in that: The following steps are involved: Providing a positive electrode plate, a sodium-based solid electrolyte layer and a negative electrode plate, wherein the material of the negative electrode plate includes metallic sodium; Performing a first surface treatment on a side of the sodium-based solid electrolyte layer facing the negative electrode plate to form a first interface improvement layer on the sodium-based solid electrolyte layer; performing a second surface treatment on a side of the negative electrode plate facing the sodium-based solid electrolyte layer to form a second interface improvement layer on the negative electrode plate; The positive electrode sheet, the sodium-based solid electrolyte layer and the negative electrode sheet are stacked; Wherein, the first surface treatment step comprises: Forming an inorganic intermediate layer on the surface of the sodium-based solid electrolyte layer, wherein the material of the inorganic intermediate layer includes one or more of PBr5, NBr3, POBr3, PI3 and NI3; forming a metal intermediate layer on the inorganic intermediate layer, wherein the material of the metal intermediate layer includes metallic sodium; Performing heat treatment under a protective atmosphere to melt the metal intermediate layer and react with the inorganic intermediate layer to obtain the first interface improvement layer; Wherein, the second surface treatment step comprises: The negative electrode plate is heated under a protective atmosphere, and is contacted with a reaction gas for reaction, wherein the reaction gas includes one or more of PF3, PF5, NF3, NOF, NO2F, OF2, O2F2, O4F2 and O5F2 to obtain the second interface improvement layer.

2. The preparation method according to claim 1, characterized in that The preparation method meets one or more of the following characteristics (1) to (2): (1) The thickness of the inorganic intermediate layer is 10 nm to 50 nm; (2) The thickness of the metal intermediate layer is 100nm~400nm.

3. The preparation method according to claim 1, characterized in that: The heat treatment is carried out at a temperature of 100° C. to 120° C. and for a time of 10 min to 60 min.

4. The preparation method according to claim 1, characterized in that: In the step of forming the second interface improvement layer, the heating temperature of the negative electrode plate is 60° C. to 80° C., and the contact reaction time of the negative electrode plate and the reaction gas is 0.5 min to 30 min.

5. The preparation method according to any one of claims 1 to 4, characterized in that The method for preparing the solid-state sodium metal battery further comprises the following steps: A third interface improvement layer is formed on the side of the positive electrode sheet facing the sodium-based solid electrolyte layer, and the material of the third interface improvement layer includes NaF, NaBr, Na3N, Na2O, NaLaCl4, Na 0.7 Zr 0.3 La 0.7 At least one of Cl4, Na3YCl6, Na3InCl6 and NaTaCl6.

6. The preparation method according to claim 5, characterized in that: The preparation method meets one or more of the following characteristics (1) to (2): (1) The positive electrode sheet includes a positive electrode current collector and a positive electrode layer disposed on the positive electrode current collector, wherein the positive electrode layer includes a positive electrode material, a sodium-based solid electrolyte, a binder and a conductive agent; and the third interface improvement layer is formed on the positive electrode layer; (2) The thickness of the third interface improvement layer is 10 nm to 40 nm.

7. The preparation method according to any one of claims 1 to 4, characterized in that The method for preparing the solid-state sodium metal battery further comprises the following steps: Adding a precursor solution between the sodium-based solid electrolyte layer and the positive electrode plate, the precursor solution containing a solvent, a sodium salt dispersed in the solvent, an α-diazo lactone, and a catalyst, wherein the catalyst is used to catalyze the ring-opening polymerization of the α-diazo lactone; The precursor solution is subjected to a heating treatment to react and form a buffer layer.

8. The preparation method according to claim 7, characterized in that: The preparation method meets one or more of the following characteristics (1) to (2): (1) The sodium salt is selected from one or more of NaTFSI and NaFSI; (2) The concentration of the sodium salt is 1 mol / L to 1.5 mol / L.

9. The preparation method according to claim 7, characterized in that: The preparation method meets one or more of the following characteristics (1) to (3): (1) The α-diazo lactone is one or more of a five-membered ring α-diazo lactone, a six-membered ring α-diazo lactone, a seven-membered ring α-diazo lactone, and an eight-membered ring α-diazo lactone; (2) the volume ratio of the α-diazo lactone to the solvent is 1:(6-10); (3) The molar ratio of the catalyst to the α-diazolactone is 1:(55-100).

10. A solid-state sodium metal battery, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 9.