Glass ceramics and crystalline articles and methods of making same

By nucleating on the surface of glass ceramic products to form a columnar crystal shell and an amorphous internal crystal structure, the problem of difficulty in balancing transparency and durability in the existing technology is solved, and glass ceramic products with high transparency and high crack resistance are realized.

CN118765265APending Publication Date: 2024-10-11CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380023992.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-07
Filing Date
2023-03-06
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

When existing glass ceramic products pursue high transparency and high durability, the homogeneous nucleation method limits the crystallinity percentage, making it difficult to balance transparency and durability, especially the contradiction between thick crystalline shells and high transparency.

Method used

By nucleating on the surface of the glass product, a columnar crystal shell is formed. The shell extends to the center of the glass ceramic product, and a crystalline shell is formed around the amorphous interior. The depth of the shell and the proportion of the amorphous interior are controlled to ensure the stability of the shell. The crystallinity and amorphous degree reach more than 99%, and the surface characteristics are optimized through heat treatment and polishing technology.

Benefits of technology

It is achieved to increase the crack resistance and sturdiness of glass ceramic products while maintaining high transparency. The matching thermal expansion coefficient of the shell layer and the amorphous interior reduces the risk of cracking, and improves transparency and crack resistance through the growth of columnar crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765265A_ABST
    Figure CN118765265A_ABST
Patent Text Reader

Abstract

Embodiments of the present disclosure relate to glass ceramic or crystalline articles. The article comprises 25 mol% < = silicon oxide < = 60 mol%, 12.5 mol% < = aluminum oxide < = 45 mol%, and 12.5 mol% < = strontium oxide < = 45 mol%. According to certain embodiments, the interior of the article is mostly amorphous glass, and the interior is at least partially surrounded by a mostly crystalline shell layer. The shell layer defines a first major surface on a first side of the interior and a second major surface opposite the first major surface on a second side of the interior. According to certain other embodiments, the article is a crystalline article in which columnar crystals grow inwardly from opposing surfaces and meet at about a midline of the article.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority under 35 U.S.C. §119 to U.S. Provisional Application No. 63 / 317,229, filed on March 7, 2022, the contents of which are incorporated herein by reference in their entirety. Background Art

[0003] Glass ceramics are partially crystalline materials that can be formed by crystallizing a portion of an amorphous glass. Crystallization can occur by some form of nucleation, such as homogeneous nucleation and heterogeneous nucleation. The unnucleated portion of the glass ceramic can be referred to as the amorphous phase, while the nucleated portion of the glass ceramic can be referred to as the crystalline phase. The crystalline phase of the glass ceramic can enhance crack resistance. Glass ceramics can be used in several applications, such as tableware, covers for electronic devices, or building products. Many glass ceramic products and methods of forming the same are not ideal for achieving the required transparency for some products and applications. Summary of the invention

[0004] In one aspect, embodiments of the present disclosure relate to a glass ceramic article. The glass ceramic article comprises 25 mol %≤silicon oxide≤60 mol %; 12.5 mol %≤aluminum oxide≤45 mol %; and 12.5 mol %≤strontium oxide≤45 mol %. The interior of the glass ceramic article is mostly amorphous glass, and the interior is at least partially surrounded by a mostly crystalline shell. The shell defines a first major surface on a first side of the interior and a second major surface on a second side of the interior opposite to the first major surface.

[0005] In one or more embodiments of the glass-ceramic article, the shell layer extends from one or both of the first major surface and the second major surface to a depth greater than or equal to 5 microns.

[0006] In one or more embodiments of the glass-ceramic article, the shell layer comprises crystals, and a majority of the crystals are formed within 15 degrees of a normal line to one or both of the first major surface and the second major surface of the glass-ceramic article.

[0007] In one or more embodiments of the glass-ceramic article, the volume of the shell layer is less than 50% of the volume of the glass-ceramic article.

[0008] In one or more embodiments of the glass-ceramic article, an absolute value of a difference between a first coefficient of thermal expansion of the inner portion and a second coefficient of thermal expansion of the shell layer is no greater than 2 μm / (m° C.).

[0009] In one or more embodiments of the glass-ceramic article, the shell layer is composed of Sr(Al2Si2O8) crystals.

[0010] In one or more embodiments of the glass-ceramic article, the aluminum oxide is present in an amount within 1 mole % of the amount of strontium oxide.

[0011] In one or more embodiments of the glass-ceramic article, the interior is at least 99% amorphous by volume and the shell is at least 99% crystalline by volume. In one or more such embodiments of the glass-ceramic article, the transition between the shell and the interior is abrupt, such that the glass-ceramic article changes from at least 99% crystalline by volume to at least 99% amorphous by volume in a distance of less than 10 microns.

[0012] In one or more embodiments of the glass-ceramic article, the glass-ceramic article comprises 1 mol % or less of other ingredients individually and 5 mol % or less of all other ingredients in total.

[0013] In one or more embodiments of the glass-ceramic article, at least 80% of light having a wavelength in the range of 400 nm to 800 nm incident on one of the first major surface or the second major surface of the glass-ceramic article is axially transmitted through the glass-ceramic article to the other of the first major surface or the second major surface.

[0014] In another aspect, an embodiment of the present disclosure relates to a glass ceramic article. The glass ceramic article includes a first crystalline shell layer extending from a first major surface of the glass ceramic article toward a center line of the glass ceramic article to a first depth. A second crystalline shell layer extends from a second major surface of the glass ceramic article toward the center line to a second depth. The second major surface is opposite to the first major surface, and the center line is in the middle of the first major surface and the second major surface. An amorphous interior is disposed between the first crystalline shell layer and the second crystalline shell layer. The first crystalline shell layer and the second crystalline shell layer have a first coefficient of thermal expansion (CTE), and the amorphous interior includes a second CTE. The absolute value of the difference between the first CTE and the second CTE is 2μm / (m℃).

[0015] In one or more embodiments of the glass-ceramic article, each of the first crystalline shell, the second crystalline shell, and the amorphous interior comprises the same composition. In one or more such embodiments, the composition comprises silicon oxide, aluminum oxide, and strontium oxide. In addition, in one or more such embodiments, the composition comprises 25 mol%≤silicon oxide≤60 mol%; 12.5 mol%≤aluminum oxide≤45 mol%; and 12.5 mol%≤strontium oxide≤45 mol%.

[0016] In one or more embodiments of the glass-ceramic article, the first depth is 5 microns to 250 microns, and wherein the second depth is 5 microns to 250 microns. In one or more such embodiments, the first depth is approximately equal to the second depth.

[0017] In one or more embodiments of the glass-ceramic article, each of the first crystalline shell layer and the second crystalline shell layer comprises columnar crystals extending from the first major surface and the second major surface, respectively. In one or more such embodiments, the columnar crystals are within 15 degrees of a normal line to the first major surface and the second major surface, respectively.

[0018] In one or more embodiments of the glass-ceramic article, the transition between at least one of the first crystalline shell or the second crystalline shell and the amorphous interior is abrupt, such that the glass-ceramic article changes from being at least 99% crystalline by volume in the first crystalline shell or the second crystalline shell to being at least 99% amorphous by volume in the amorphous interior within a distance of less than 10 microns.

[0019] In one or more embodiments of the glass ceramic article, at least 80% of light having a wavelength range of 400nm to 800nm ​​incident on one of the first major surface or the second major surface of the glass ceramic article is axially transmitted through the glass ceramic article to the other of the first major surface or the second major surface.

[0020] In yet another aspect, embodiments of the present disclosure relate to a method of making a glass-ceramic article. In the method, columnar crystals nucleate at the surface of the glass article to form a crystalline shell around an amorphous interior. The columnar crystals extend to a depth of at least 5 microns in the glass-ceramic article.

[0021] In one or more embodiments of the method, nucleation involves heat treating the glass article at a temperature of 1010° C. to 1080° C. In one or more such embodiments, the heat treatment is performed for a period of 1 hour to 5 hours. Additionally, in one or more such embodiments, after the heat treatment, the surface is polished by grinding a portion of the crystallized shell layer.

[0022] In one or more embodiments of the method, the crystalline crust has a depth of up to 250 microns.

[0023] In one or more embodiments of the method, prior to nucleation, the method further involves forming a glass article from a glass composition comprising 25 mol %≤silicon oxide≤60 mol %, 12.5 mol %≤aluminum oxide≤45 mol %, and 12.5 mol %≤strontium oxide≤45 mol %.

[0024] In one or more embodiments of the method, the crystalline shell has a first coefficient of thermal expansion (CTE) and the amorphous interior has a second CTE. The absolute value of the difference between the first CTE and the second CTE is 2 μm / (m° C.).

[0025] In one or more embodiments of the method, the columnar crystals are within 15 degrees of a normal to the surface.

[0026] In one or more embodiments of the method, the transition between the crystalline shell and the amorphous interior is abrupt such that the glass-ceramic article changes from being at least 99 vol% crystalline in the crystalline shell to being at least 99 vol% amorphous in the amorphous interior over a distance of less than 10 microns.

[0027] According to another aspect, embodiments of the present disclosure relate to a crystalline article. The crystalline article comprises 40 mol% ≤ SiO2 ≤ 50 mol%, 25 mol% ≤ Al2O3 ≤ 32.5 mol%, and 22.5 mol% ≤ SrO ≤ 30 mol%. In one or more embodiments, Al2O3 ≥ SrO. Additionally, in one or more embodiments, the crystalline article comprises at least 90 vol% of crystalline material, and the crystalline material comprises 90 vol% of a single crystal phase.

[0028] In one or more embodiments, the crystalline article includes a first major surface and a second major surface, where the second major surface is opposite the first major surface. In one or more such embodiments, the distance between the first major surface and the second major surface defines the thickness of the crystalline article, and the thickness is at most 1 millimeter (mm).

[0029] In one or more such embodiments, the crystalline article is composed of columnar crystals, where most of the columnar crystals are oriented within 15 degrees of the normal to one or both of the first major surface and the second major surface.

[0030] In one or more embodiments, the single crystal phase is Sr(Al2Si2O8). Additionally, in one or more embodiments, the crystalline phase includes 1 vol% or less of a secondary crystalline phase. In one or more such embodiments, the secondary phase is SrSiO3.

[0031] In one or more embodiments of the crystalline article, the crystalline article transmits at least 70% of light having a wavelength of 400 nm to 800 nm.

[0032] In one or more embodiments of the crystalline article, the composition of the crystalline article includes 0 < Al2O3 – SrO ≤ 5 mol%. In one or more embodiments of the crystalline article, the crystalline article includes other components individually at 1 mol% or less and all other components in total at 5 mol% or less.

[0033] In one or more embodiments, the crystalline article includes a first crystalline region extending from the first major surface into the thickness and a second crystalline region extending from the second major surface into the thickness, and the first crystalline region and the second crystalline region meet at approximately the midpoint of the thickness.

[0034] According to another aspect, an embodiment of the present disclosure relates to a crystalline article. The crystalline article includes 40 mol% to 50 mol% of SiO2, as well as Al2O3 and SrO. In this composition, Al2O3 and SrO are provided such that 0 < Al2O3 – SrO ≤ 5 mol%. The crystalline article has a first major surface, a second major surface, and a thickness, and the second major surface is opposite the first major surface. The thickness is the distance between the first major surface and the second major surface, and the thickness is 1 mm or less.

[0035] In one or more embodiments, the crystalline article includes SiO2 + Al2O3 + SrO ≥ 85 mol%. In one or more embodiments, the crystalline article is composed of at least 90 vol% of a crystalline phase. In one or more such embodiments, the crystalline phase includes at least 90 vol% of a first crystal structure, particularly Sr(Al2Si2O8). Additionally, in one or more such embodiments, the crystalline phase includes no more than 1 vol% of a second crystal structure, particularly SrSiO3.

[0036] In one or more embodiments of the crystalline article, the crystalline article includes a first crystallization zone and a second crystallization zone. The first crystallization zone includes columnar crystals extending from the first major surface toward the midpoint of the thickness, and the second crystallization zone includes columnar crystals extending from the second major surface toward the midpoint of the thickness. In one or more such embodiments, the columnar crystals are oriented within 15° of the normal to the respective first major surface and second major surface.

[0037] In one or more embodiments, at least 70% of the light having a wavelength range of 400 nm to 800 nm incident on one of the first major surface or the second major surface of the crystalline article transmits through the crystalline article to the other of the first major surface or the second major surface.

[0038] According to yet another aspect, an embodiment of the present disclosure relates to a method of manufacturing a crystalline article. In this method, first columnar crystals on the first major surface of a glass article and second columnar crystals on the second major surface of the glass article are nucleated until the first columnar crystals and the second columnar crystals meet to form a crystalline article. Both the first columnar crystals and the second columnar crystals extend inward from the respective first major surface and second major surface. The glass article includes SiO2, Al2O3, and SrO, where 40 mol% ≤ SiO2 ≤ 50 mol% and 0 ≤ Al2O3 – SrO ≤ 5 mol%.

[0039] In one or more embodiments of the method, the crystals are nucleated by heat-treating the glass article at a temperature of 1010 °C to 1080 °C. In one or more such embodiments, the heat treatment is carried out for 1 hour to 5 hours.

[0040] In one or more embodiments, after the heat treatment, at least one of the first major surface or the second major surface is polished by grinding a portion of at least one of the first major surface or the second major surface.

[0041] In one or more embodiments of the method, the thickness is 1 mm or less.

[0042] In one or more embodiments of the method, the first columnar crystals and the second columnar crystals contain at least 90% by volume of a first crystal structure, in particular Sr(Al2Si2O8). In addition, in one or more embodiments, the first columnar crystals and the second columnar crystals contain 1% by volume or less of a second crystal structure, in particular SrSiO3.

[0043] In one or more embodiments, the glass article comprises 25 mol %≤Al2O3≤32.5 mol %, and 22.5 mol %≤SrO≤30 mol %.

[0044] Additional aspects of the present disclosure are described in the detailed description. Those skilled in the art will readily understand some aspects related to the present disclosure from the detailed description, drawings and claims. The summary of the invention and the following detailed description are exemplary and construct a framework to facilitate understanding of the essence of the claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] The accompanying drawings of the present disclosure promote further understanding of the claims. The accompanying drawings show one or more aspects of the innovative technology of the present disclosure. The accompanying drawings can be further elaborated through additional descriptions of the detailed description.

[0046] Figure 1A is a schematic side view of a glass-ceramic article according to an embodiment of the present disclosure.

[0047] Figure 1B is a digital image of a glass-ceramic article from a top-down perspective of the glass-ceramic article according to the innovative aspects of the present disclosure;

[0048] Figure 2 is a thermal expansion graph of an amorphous glass-ceramic article according to innovative aspects of the present disclosure.

[0049] Figure 3 is a thermal expansion graph of a crystalline article according to innovative aspects of the present disclosure.

[0050] Figure 4 is a graph of differential scanning thermal analysis readings as a function of temperature for a nucleated article according to innovative aspects of the present disclosure.

[0051] Figure 5is a digital image of a glass-ceramic article from a cross-sectional view of glass that has been nucleated at 1050° C. for 1 hour and 3 minutes in accordance with innovative aspects of the present disclosure.

[0052] Figure 6 is a digital image of a glass-ceramic article from a cross-sectional view of glass that has been nucleated at 1050° C. for 2 hours and 33 minutes in accordance with innovative aspects of the present disclosure.

[0053] Figure 7 is a digital image of a glass-ceramic article from a cross-sectional view of glass that has been nucleated at 1050° C. for 3 hours and 45 minutes in accordance with innovative aspects of the present disclosure.

[0054] Figure 8 is a digital image of a glass-ceramic article from a cross-sectional view of glass that has been nucleated at 1050° C. for 4 hours and 36 minutes in accordance with innovative aspects of the present disclosure.

[0055] Fig. 9 is a digital image of a glass-ceramic article from a cross-sectional view of a glass having a shell thickness of 130 microns and an amorphous interior thickness of 540 microns in accordance with innovative aspects of the present disclosure.

[0056] Fig.10 Graphs of total transmittance versus wavelength for a completely amorphous glass article, a glass-ceramic article, and a completely crystalline article in accordance with innovative aspects of the present disclosure.

[0057] Fig.11 Graphs of axial transmittance versus wavelength for a completely amorphous glass article, a glass-ceramic article, and a completely crystalline article in accordance with innovative aspects of the present disclosure.

[0058] Fig.12 Graphs of diffuse transmittance versus wavelength for a fully amorphous glass article, a glass-ceramic article, and a fully crystalline article in accordance with innovative aspects of the present disclosure.

[0059] Fig.13 2 is a graph of scattering versus wavelength for a completely amorphous glass article, a glass-ceramic article, and a completely crystalline article in accordance with innovative aspects of the present disclosure.

[0060] Fig.14 is an X-ray diffraction intensity versus 2θ plot of a glass-ceramic article according to inventive aspects of the present disclosure.

[0061] Fig.15 is a digital image of an indentation on a surface of a glass-ceramic article from a top view of the glass-ceramic article, the glass-ceramic article being heat treated for 4 hours and 36 minutes, according to innovative aspects of the present disclosure.

[0062] Fig.16 is a digital image of an indentation on a surface of a glass-ceramic article from a top view of the glass-ceramic article, the glass-ceramic article being heat treated for 2 hours and 30 minutes, according to innovative aspects of the present disclosure.

[0063] Fig.17 Depicted are stages in forming a crystalline article from an amorphous glass article according to an exemplary embodiment of the present disclosure.

[0064] Figures 18 to 21 depicts SEM micrographs of crystallized products having thicknesses of 0.53 mm, 1.00 mm, 1.03 mm, and 1.17 mm;

[0065] Fig. 22 Depiction Fig.18 Elemental dispersion spectrum scan of the crystalline phase of the crystalline product.

[0066] Fig.23 Depiction Fig.21 Elemental dispersion spectroscopy scans of two different crystalline phases of the crystalline product.

[0067] Fig.24 Plotting the X-ray diffraction spectrum of the single crystalline phase found in samples less than 1 mm thick.

[0068] Fig.25 X-ray diffraction spectra depicting the two crystalline phases present in samples with a thickness greater than 1 mm.

[0069] Fig.26 Graph showing the change in transmittance of a crystalline article at thicknesses of 0.40 mm, 0.87 mm, and 1.0 mm as a function of wavelength.

[0070] Fig. 27 Graph showing changes in transmittance with wavelength for a crystalline product having a single crystal and a thickness of 0.40 mm, a single crystal phase and a thickness of 1.0 mm, and a polycrystalline phase and a thickness of 1.0 mm.

[0071] Fig.28 SEM micrograph depicting the crack path produced by the Vickers indenter.

[0072] Fig.29 A crystalline article according to an embodiment of the present disclosure is depicted, demonstrating the transparency of the crystalline article.

[0073] Fig.30 Describes an exemplary embodiment according to the present disclosure Fig.29 Micrograph of a crystallized product showing a columnar crystal structure. DETAILED DESCRIPTION

[0074] The present disclosure is not limited to the aspects or methods described in the specific embodiments or shown in the drawings and / or described in relation to the drawings described herein. Those skilled in the art will understand that the aspects described in the specific embodiments or shown in the drawings may be interrelated or applicable to other aspects seen elsewhere in the specific embodiments and / or drawings.

[0075] There is a great demand for glass ceramics and crystalline products with both high transparency and high durability. The common method for making glass ceramics at present is to form glass ceramics by homogeneous nucleation, wherein nucleation occurs at the surface away from the system. However, forming glass ceramics by homogeneous nucleation often requires limiting the percentage of crystallinity to achieve high transparency, because the crystal orientation in the shell of homogeneous nucleation glass ceramics is not conducive to transparency. In order to prevent high light scattering, limiting the percentage of crystallinity may result in an extremely thin shell, wherein high light scattering reduces transparency. However, higher crystallinity is associated with higher durability, so from the perspective of durability, a thicker crystalline shell is desired. Therefore, it is necessary to include a thick crystalline shell or even a fully crystalline material while maintaining high transparency and preventing crack propagation.

[0076] As used herein, "most" and "mostly" mean greater than 50%. In addition, "most" or "mostly" attributes or characteristics can be further reduced to at least 90%, such as at least 99% of the attributes or characteristics, such as the crystallinity of the shell, the amorphous degree of the interior, and the orientation of the shell crystals.

[0077] For the purposes of this disclosure, total transmittance is equal to diffuse transmittance plus axial transmittance. In addition, for the purposes of this disclosure, "transmittance" generally refers to "total transmittance", and therefore, unless otherwise stated, both "transmittance" and "total transmittance" refer to the orthodox understanding of the definition (such as defined in "ASTM International"). Axial transmittance is the transmittance of light through a material, where the light maintains its route through the material and reaches the reader of the detector. Diffuse transmission occurs when light deviates in different directions when passing through the material due to phenomena such as seed crystals, bubbles or turbidity. The transmittance of a glass-ceramic article is measured by placing the article in a collecting sphere detector. For axial transmittance, the article is placed at a certain distance from the detector so that the light that passes through the material is recorded as the light that maintains its route through the material to the detector, and the detector records almost no (ideally zero) scattered light that passes through the material (because the scattered light will deviate from the detector when the detector is placed far enough away from the material / sample). Diffuse transmittance is measured by removing the plug from the collecting sphere so that axial light (light that maintains its path through the article) exits the sphere and enters the light trap, so that the remaining light recorded by the sphere collector is diffuse light (light that deviates from its path while passing through the article).

[0078] like Figure 1A As depicted, in the present disclosure, a glass-ceramic article 100 includes a shell 110 and an amorphous interior 120. The amorphous interior 120 mostly includes amorphous glass, and the shell 110 mostly includes crystals. As used herein, the shell 110 and the amorphous interior 120 may be collectively referred to as a composite material.

[0079] Shell 110 can be viewed as a layer of columnar crystals, wherein the crystals are interconnected to form shell 110, wherein individual crystals have a length and a width orthogonal thereto. In aspects of the present disclosure, the length of an individual crystal is greater than or equal to twice the width of the crystal, such as a length greater than or equal to ten times the width, a length greater than or equal to twenty times the width, and a length greater than or equal to fifty times the width.

[0080] The shell 110 at least partially or completely surrounds the amorphous interior 120. In one or more embodiments, "surrounding" means that the shell 110 encloses the amorphous interior 120 and the amorphous interior 120 does not enclose the shell 110, and / or means that any curvature in the amorphous interior 120 includes the shell 110 being formed around the curvature of the amorphous interior 120 and does not include the amorphous interior 120 being formed around the shell 110, and / or means that the amorphous interior 120 is sandwiched between the shells 110 and the shells 110 are not sandwiched between the amorphous interiors 120. Including the amorphous interior 120 can have a substantial effect on improving the transparency of the glass-ceramic article 100, wherein the combination of the shell 110 and the amorphous interior 120 can produce a glass-ceramic article 100 with a higher total transmittance than a corresponding crystalline article, wherein the columnar crystals of the shell extend all the way to the center of the article, thus without the amorphous interior. Therefore, when considering only the goal of increasing transparency for embodiments having at least a certain shell depth, it is more desirable to stop columnar crystal growth before the crystals meet the center of the glass article. Nevertheless, as will be discussed below, embodiments of the present disclosure also relate to fully crystalline articles.

[0081] The glass ceramic article 100 includes a first major surface 130 and a second major surface 140 opposite the first major surface 130. A minor surface 150 connects the first major surface 130 and the second major surface 130. The first major surface 130 and the second major surface 140 define a thickness T1 of the glass ceramic article 100. For the purposes of the present disclosure, the shell depth D refers to the distance that the shell 110 extends from one of the first major surface 130 or the second major surface 140 of the glass ceramic article 100 toward the centerline 160 of the glass ceramic article 100. Typically, the shell depth D will be less than half of the thickness T1 of the glass ceramic article 100. That is, in contrast to the fully crystallized embodiment described below, the columnar crystals extend from each of the first major surface 130 and the second major surface 140 and do not meet at the centerline 160 of the glass ceramic article 100. The thickness T2 of the amorphous inner portion 120 is the thickness T1 of the glass-ceramic article 100 minus the depth D of each shell layer 110 a , 110 b , ie, T2 = T1 −2D.

[0082] The shell 110 may be formed by heterogeneous nucleation without a nucleating agent. In other words, and more specifically, the shell 110 may be surface nucleated, for example, from defects on the surface, to promote inward crystal growth, thereby producing columnar crystals oriented perpendicular or nearly perpendicular to the respective surfaces 130, 140, 150. The perpendicular or nearly perpendicular orientation of the crystals in the shell may produce higher transparency and improved radial crack resistance in the shell 110 compared to, for example, randomly oriented crystals. The amorphous interior may also have high transparency because the interior mostly contains a glassy amorphous composition.

[0083] The glass-ceramic article 100 can be formed into a variety of sizes and shapes. In aspects of the present disclosure, the glass-ceramic article 100 can be a rectangular article, wherein the amorphous interior 120 is at least partially sandwiched between the top shell layer 110a and the bottom shell layer 110b. In aspects of the present disclosure, the glass-ceramic article 100 can be a spherical article, such as a sphere or an ellipsoid, wherein the shell layer 110 at least partially surrounds the amorphous interior 120. In aspects of the present disclosure, the glass-ceramic article 100 can have a combination of spherical and flat surfaces, such as a hemisphere, wherein the shell layer 110 at least partially surrounds the amorphous interior 120. In aspects of the present disclosure, the glass-ceramic article 100 can be a sheet, wherein the shell layers form the major surfaces 130, 140 of the sheet, such as Figure 1A As depicted. The sheet can have significant advantages, such as being used as a transparent outer cover for devices such as mobile phone devices. In aspects of the present disclosure, the thickness T1 of the glass-ceramic article 100 sheet can be greater than 10 microns, such as greater than 50 microns or greater than 100 microns. Increasing the thickness of the sheet can increase the robustness of the sheet for use in applications requiring a stronger and / or more durable transparent outer cover.

[0084] Shell 110 may be mostly crystalline, i.e., mostly composed of crystals. In aspects of the present disclosure, shell 110 may be at least 99% crystalline. In aspects of the present disclosure, shell 110 may be at least 90% crystalline. The higher the crystallinity of shell 110 and / or the greater the depth D of shell 110 may result in lower transparency or transmittance. The higher the crystallinity of shell 110 and / or the greater the depth D of shell 110 may result in higher robustness of shell 110. In aspects of the present disclosure, amorphous interior 120 may be at least 99% amorphous by volume. In aspects of the present disclosure, amorphous interior 120 may be at least 90% amorphous by volume. The higher the amorphousness of amorphous interior 120 and / or the greater the thickness T2 of amorphous interior 120 may result in greater transparency of glass ceramic article 100.

[0085] Ideally, the crystals 170 of the shell layer grow perpendicular to a surface of the shell layer 110 (e.g., the first major surface 130 or the second major surface 140) and the crystals extend from the surface. The crystals 170 of the shell layer may not grow completely perpendicular to the surface of the shell layer 110. The crystals 170 may grow approximately completely (even if not completely) perpendicular to the surface of the shell layer 110. The crystals 170 may grow at a very small angle from the normal direction of the surface of the shell layer 110, such as 0.5 degrees from the normal to the surface from which the crystals 170 extend. Other crystals 170 may grow at a significantly larger angle from the normal direction of the surface of the shell layer 110, such as 15 degrees from the normal to the surface from which the crystals 170 extend.

[0086] In one or more embodiments, the shell 110 and the amorphous interior 120 have similar coefficient of thermal expansion (CTE) values. Advantageously, closely matching the CTE values ​​of the amorphous interior 120 and the shell 110 can help prevent cracking of the glass-ceramic article 100. In one or more embodiments, the less mismatch in CTE values ​​between the amorphous interior 120 and the shell 110, the less likely the glass-ceramic article 100 is to crack during manufacturing. Figure 2 and Figure 3 The CTE values ​​of exemplary embodiments of the amorphous interior 120 and the crystalline shell 110 of the glass-ceramic article 100 are depicted, respectively. Figure 2 It can be seen that the CTE of the amorphous interior 120 is about 5.76 μm / (m°C) between about 25°C and about 300°C. Figure 3It can be seen that the CTE of the crystalline shell 110 is about 5.75 μm / (m°C) between the same temperature range. For the crystalline shell 110, the CTE is measured in the direction parallel to the crystal growth direction (i.e., perpendicular to the surface of the crystalline shell 110). Therefore, in the exemplary embodiment, the CTE difference (absolute value) between the crystalline shell 110 and the amorphous interior 120 is only 0.01 μm / (m°C). In one or more embodiments, the CTE difference (absolute value) between the crystalline shell 110 and the amorphous interior 120 is 2 μm / (m°C) or less, 1 μm / (m°C) or less, 0.5 μm / (m°C or less, 0.2 μm / (m°C) or less, 0.1 μm / (m°C) or less, 0.05 μm / (m°C) or less, 0.02 μm / (m°C) or less, or 0.01 μm / (m°C) or less. In one or more embodiments, the CTE values ​​of the crystalline shell 110 and the amorphous interior 120 are the same (i.e., the difference is 0 μm / (m°C)).

[0087] The glass-ceramic article 100 of the present disclosure may have a thickness T1 of 5 mm or less, such as 5 micrometers or more and 10 micrometers or less, 5 micrometers or more and 50 micrometers or less, 5 micrometers or more and 100 micrometers or more, 5 micrometers or more and 500 micrometers or less, 5 micrometers or more and 1 mm or more, 5 micrometers or more and 5 mm or more, 50 micrometers or more and 100 micrometers or more, 50 micrometers or more and 500 micrometers or less, 50 micrometers or more and 1 mm or more, 50 micrometers or more and 500 micrometers or less, 50 micrometers or more and 1 mm or more, 50 micrometers or more and 500 micrometers or less, 50 micrometers or more and 1 mm or more, 50 micrometers or more and 500 micrometers or less, and any sub-range formed by any of the foregoing starting points and / or endpoints provided herein.

[0088] Transparency can be measured by determining the transmittance of the glass, where transmittance is the fraction of incident light that moves through the sample, and is therefore usually measured as a percentage, where high transmittance is equivalent to high transparency and low transmittance is equivalent to low transparency. Transmittance can depend on various factors, such as the wavelength of light passing through the glass-ceramic article or the thickness of the glass-ceramic article. For example, the larger the wavelength of light passing through the glass-ceramic article, the higher the transmittance of light of that wavelength when passing through the article; for another example, the greater the thickness of the glass-ceramic article, the lower the transmittance of light when passing through the article of that thickness. The Beer-Lambert law describes the relationship between thickness and transmittance with the equation -log(T) = εlc, where T is the transmittance through the sample, ε is the molar attenuation coefficient of the species of the sample, c is the concentration of the species, and l is the optical path length or sample thickness. According to the Beer-Lambert law, it is obvious that the transmittance of a sample (such as a glass-ceramic article) decreases as the thickness of the glass-ceramic article increases, and the transmittance of a sample (such as a glass-ceramic article) increases as the thickness of the glass-ceramic article decreases. Therefore, a glass-ceramic article with a thin thickness, such as 5 microns, can give a higher transparency. However, thicker glass ceramic articles, such as 1 mm, can provide greater robustness and / or crack resistance. In one or more embodiments, the thickness T1 of the glass ceramic article does not exceed 5 mm to balance robustness and transparency. Nevertheless, embodiments of the present disclosure extend to glass ceramic articles having a thickness greater than 5 mm and / or a transmittance less than 50%.

[0089] In aspects of the present disclosure, the shell 110 may be completely crystalline or at least 99% crystalline, wherein the crystal growth of the glass is oriented perpendicular to the surface and may extend to about half of the thickness or volume of the glass-ceramic article 100. In aspects of the present disclosure, the amorphous interior 120 may be completely amorphous or at least 99% amorphous, wherein the glass-ceramic article 100 has little or no crystallization. In one or more embodiments, the transition between the shell 110 and the amorphous interior 120 is abrupt, so that the glass-ceramic article 100 changes from at least 99% crystalline by volume to at least 99% amorphous by volume within a distance of no more than 10 microns, no more than 5 microns, or no more than 1 micron. Because some conventional glass-ceramic articles tend to have a large CTE difference between the crystalline phase and the amorphous phase, it is difficult to achieve this abrupt transition without defects in the glass-ceramic article. Such conventional glass-ceramic articles with abrupt transitions may be more prone to cracking and / or defects during nucleation. According to the present disclosure, the composition of the glass-ceramic article 100 is prepared to provide a glass-ceramic article 100 that provides an abrupt transition between the crystalline shell 110 and the amorphous interior 120. Specifically, the composition of the present disclosure is based on silicon oxide (SiO2), aluminum oxide (Al2O3) and strontium oxide (SrO) in the following ranges.

[0090] In the present disclosure, silicon oxide, aluminum oxide, and strontium oxide (collectively referred to as "major components") may comprise the majority of the components of the glass-ceramic article. In one or more embodiments, the major components account for at least 80 mol% of the glass-ceramic article 100, at least 85 mol% of the glass-ceramic article 100, at least 90 mol% of the glass-ceramic article 100, at least 95 mol% of the glass-ceramic article 100, or up to 100 mol% of the glass-ceramic article 100. In one or more embodiments, the glass-ceramic article 100 comprises 80 mol% to 100 mol%, 80 mol% to 95 mol%, 80 mol% to 90 mol%, 80 mol% to 85 mol%, 85 mol% to 100 mol%, 85 mol% to 95 mol%, 85 mol% to 90 mol%, 90 mol% to 100 mol%, 90 mol% to 95 mol%, 95 mol% to 100 mol%, or any range or sub-range of the major component amount between the aforementioned endpoints.

[0091] In one or more embodiments, the glass ceramic article 100 may include an amount of silicon oxide (SiO2) in the following ranges: 25 mol% ≤ silicon oxide ≤ 60 mol%, 25 mol% ≤ silicon oxide ≤ 55 mol%, 25 mol% ≤ silicon oxide ≤ 50 mol%, 25 mol% ≤ silicon oxide ≤ 45 mol%, 25 mol% ≤ silicon oxide ≤ 40 mol%, 25 mol% ≤ silicon oxide ≤ 35 mol%, 25 mol% ≤ silicon oxide ≤ 30 mol%, 30 mol% ≤ silicon oxide ≤ 60 mol%, 30 mol% ≤ silicon oxide ≤ 55 mol%, 30 mol% ≤ silicon oxide ≤ 50 mol%, 30 mol% ≤ silicon oxide ≤ 50 mol%, 30 mol% ≤ silicon oxide ≤ 45 mol%, 30 mol% ≤ silicon oxide ≤ 40 mol%, 30 mol% ≤ silicon oxide ≤ 35 mol%, 35 mol% ≤ silicon oxide ≤ 35 mol%, 35 mol% ≤ silicon oxide ≤ 30 mol%, 30 mol% ≤ silicon oxide ≤ 60 mol%, 30 mol% ≤ silicon oxide ≤ 55 mol%, 30 mol% ≤ silicon oxide ≤ 50 mol%, 30 mol% ≤ silicon oxide ≤ 50 mol%, 30 mol% ≤ silicon oxide ≤ 45 mol%, 30 mol% ≤ silicon oxide ≤ 40 mol%, 30 mol% ≤ silicon oxide ≤ 35 mol%, 35 mol% ≤ silicon oxide ≤ 35 mol%. %≤silicon oxide≤60 mol%, 35 mol%≤silicon oxide≤55 mol%, 35 mol%≤silicon oxide≤50 mol%, 35 mol%≤silicon oxide≤45 mol%, 35 mol%≤silicon oxide≤40 mol%, 40 mol%≤silicon oxide≤60 mol%, 40 mol%≤silicon oxide≤55 mol%, 40 mol%≤silicon oxide≤50 mol%, 40 mol%≤silicon oxide≤45 mol%, 45 mol%≤silicon oxide≤60 mol%, 45 mol%≤silicon oxide≤55 mol%, 45 mol%≤silicon oxide≤50 mol%, 50 mol%≤silicon oxide≤60 mol%, 50 mol%≤silicon oxide≤55 mol%, 55 mol%≤silicon oxide≤60 mol%, and any ranges or sub-ranges formed by any of the foregoing starting points and / or endpoints provided herein.

[0092] In aspects of the present disclosure, the glass-ceramic article may include 12.5 mol%≤alumina≤45 mol% aluminum oxide (Al2O3), such as 12.5 mol%≤alumina≤40 mol%, 12.5 mol%≤alumina≤35 mol%, 12.5 mol%≤alumina≤30 mol%, 12.5 mol%≤alumina≤25 mol%, 12.5 mol%≤alumina≤20 mol%, 12.5 mol%≤alumina≤15 mol%, 17.5 mol%≤alumina≤45 mol%, 17.5 mol%≤alumina≤40 mol%, 17.5 mol%≤alumina≤35 mol%, 17.5 mol%≤alumina≤30 mol%, 17.5 mol%≤alumina≤30 mol%, 17.5 mol%≤alumina≤25 mol%, 17.5 mol%≤alumina≤20 mol%, 22.5 mol%≤alumina Alumina ≤ 45 mol%, 22.5 mol% ≤ alumina ≤ 40 mol%, 22.5 mol% ≤ alumina ≤ 35 mol%, 22.5 mol% ≤ alumina ≤ 30 mol%, 22.5 mol% ≤ alumina ≤ 25 mol%, 27.5 mol% ≤ alumina ≤ 45 mol%, 27.5 mol% ≤ alumina ≤ 40 mol%, 27.5 mol% ≤ alumina ≤ 35 mol%, 27.5 mol% ≤ alumina ≤ 30 mol%, 32.5 mol% ≤ alumina ≤ 45 mol%, 32.5 mol% ≤ alumina ≤ 40 mol%, 32.5 mol% ≤ alumina ≤ 35 mol%, 37.5 mol% ≤ alumina ≤ 45 mol%, 37.5 mol% ≤ alumina ≤ 40 mol%, 42.5 mol% ≤ alumina ≤ 45 mol%, or any ranges and sub-ranges formed by any of the foregoing starting points and / or endpoints provided herein.

[0093] In aspects of the present disclosure, the glass-ceramic article may include 12.5 mol% ≤ strontium oxide ≤ 45 mol% strontium oxide (SrO), such as 12.5 mol% ≤ strontium oxide ≤ 40 mol%, 12.5 mol% ≤ strontium oxide ≤ 35 mol%, 12.5 mol% ≤ strontium oxide ≤ 30 mol%, 12.5 mol% ≤ strontium oxide ≤ 25 mol%, 12.5 mol% ≤ strontium oxide ≤ 20 mol%, 12.5 mol% ≤ strontium oxide ≤ 15 mol%, 12.5 mol% ≤ strontium oxide ≤ 20 mol%, 12.5 mol% ≤ strontium oxide ≤ 25 ... %≤15 mol% of strontium oxide, 17.5 mol%≤45 mol% of strontium oxide, 17.5 mol%≤40 mol% of strontium oxide, 17.5 mol%≤35 mol% of strontium oxide, 17.5 mol%≤30 mol% of strontium oxide, 17.5 mol%≤30 mol% of strontium oxide, 17.5 mol%≤25 mol% of strontium oxide, 17.5 mol%≤20 mol% of strontium oxide, 22.5 mol% ≤ strontium oxide ≤ 45 mol%, 22.5 mol% ≤ strontium oxide ≤ 40 mol%, 22.5 mol% ≤ strontium oxide ≤ 35 mol%, 22.5 mol% ≤ strontium oxide ≤ 30 mol%, 22.5 mol% ≤ strontium oxide ≤ 25 mol%, 27.5 mol% ≤ strontium oxide ≤ 45 mol%, 27.5 mol% ≤ strontium oxide ≤ 40 mol%, 27.5 mol% ≤ strontium oxide ≤ 35 mol%, 27.5 mol% ≤ Strontium oxide ≤30 mol%, 32.5 mol% ≤ strontium oxide ≤45 mol%, 32.5 mol% ≤ strontium oxide ≤40 mol%, 32.5 mol% ≤ strontium oxide ≤35 mol%, 37.5 mol% ≤ strontium oxide ≤45 mol%, 37.5 mol% ≤ strontium oxide ≤40 mol%, 42.5 mol% ≤ strontium oxide ≤45 mol%, or any sub-range formed by any of the foregoing starting points and / or endpoints provided herein.

[0094] In aspects of the present disclosure, the glass ceramic article may further include a minor component, which is a component that is present in the glass ceramic article in an amount of 1 mol % or less, 0.5 mol % or less, 0.2 mol % or less, 0.1 mol % or less, or 0.05 mol % or less alone. The total amount of minor components (all minor components added up) may be present in the glass ceramic article in an amount of 5 mol % or less, 2 mol % or less, 1 mol % or less, 0.5 mol % or less, 0.2 mol % or less, or 0.1 mol % or less. In aspects of the present disclosure, the minor component may be magnesium oxide, calcium oxide, barium oxide, sodium oxide, potassium oxide, iron oxide and / or titanium oxide, etc. In one or more embodiments, the composition of the glass ceramic article may contain up to 5 mol % of boron oxide (BO) amount, such as about 1 mol % to 5 mol %, without affecting the expected properties of the glass ceramic article.

[0095] In aspects of the present disclosure, compositions particularly suitable for use in glass-ceramic articles include the following ranges of silicon oxide (SiO2), aluminum oxide (Al2O3), and strontium oxide (SrO): 40 mol% ≤ silicon oxide <50 mol%, 25 mol% ≤ aluminum oxide <35 mol%, and 25 mol% ≤ strontium oxide <35 mol%; 41 mol% ≤ silicon oxide <50 mol%, 26 mol% ≤ aluminum oxide <35 mol%, and 26 mol% ≤ strontium oxide <35 mol%; 42 mol% ≤ silicon oxide <50 mol%, 27 mol% ≤ aluminum oxide <35 mol%, and 27 mol% ≤ strontium oxide <35 mol%; 43 mol% ≤ silicon oxide <50 mol%, 28 mol% ≤ aluminum oxide <35 mol%, and 28 mol% ≤ strontium oxide <35 mol%. %≤ strontium oxide <35 mol %; 43 mol %≤ silicon oxide <50 mol %, 28.5 mol %≤ aluminum oxide <35 mol % and 28.5 mol %≤ strontium oxide <35 mol %; 43 mol %≤ silicon oxide <50 mol %, 27.5 mol %≤ aluminum oxide <35 mol % and 27.5 mol %≤ strontium oxide <35 mol %; 43 mol %≤ silicon oxide <50 mol %, 27 mol %≤ aluminum oxide <35 mol % and 27 mol %≤ strontium oxide <35 mol %; 43 mol %≤ silicon oxide <50 mol %, 27 mol %≤ aluminum oxide <35 mol % and 27 mol %≤ strontium oxide <35 mol %; 43 mol %≤ silicon oxide <50 mol %, 26.5 mol %≤ aluminum oxide <35 mol % and 26.5 mol %≤ strontium oxide <35 mol %; and or any sub-range formed by any of the foregoing starting points and / or endpoints provided herein. In one or more embodiments, in the composition of the glass-ceramic article, the amount of aluminum oxide is approximately equal to the amount of strontium oxide (e.g., within about 1 mol % difference). Additionally, in one or more embodiments, the amount of aluminum oxide and strontium oxide are both less than the amount of silicon oxide, and in particular, each is at least about 5 mol%, about 10 mol%, or about 12 mol% less than the amount of silicon oxide.

[0096] In aspects of the present disclosure, the transmittance of visible light (e.g., light in the wavelength range of 400nm to 800nm) in the amorphous interior may be higher than the transmittance of visible light in the crystalline shell; therefore, the amorphous interior may be more transparent in the visible light spectrum than the crystalline shell. Thus, in aspects of the present disclosure, at a certain glass-ceramic article thickness, when the shell thickness decreases relative to the thickness of the amorphous interior, the transparency of the glass-ceramic article may increase. When the shell surrounds the amorphous interior, even at least partially surrounding it, the transparency of the article can also be considered in terms of the relative volume of the shell compared to the volume of the amorphous interior, wherein at a certain glass-ceramic article thickness, when the shell volume decreases relative to the volume of the amorphous interior, the transmittance or transparency of the glass-ceramic article can be improved.

[0097] The volume of the shell layer and / or the volume of the amorphous interior relative to the volume of the glass-ceramic article is related to the transparency of the glass-ceramic article. For a glass-ceramic article of a particular size, an increase in the volume of the amorphous interior or a decrease in the volume of the crystalline shell layer relative to the volume of the glass-ceramic article can increase the transparency of the glass-ceramic article. In aspects of the present disclosure, the amorphous interior can be greater than 0% of the volume of the glass-ceramic article, but less than 100% of the volume of the glass-ceramic article. In one or more embodiments, the percentage of the amorphous interior by volume of the glass-ceramic article ranges from 10% to <100%, 20% to <100%, 30% to <100%, 40% to <100%, 50% to <100%, 60% to <100%, 70% to <100%, 80% to <100%, 90% to <100%, 10% to 90%, 20% to 90%, 30% to 90%, 40% to 90%, 50% to 90%, 60% to 90%, 70% to 90%, 80% to 90%, 10% to 80%, 20% to 80%, 30% to 80%, 40% to 80%, 50% to <100%, 60% to <100%, 70% to <100%, 80% to <100%, 90% to <100%, 10% to 90%, 20% to 90%, 30% to 90%, 40% to 80%, 50% to <100%, % to 80%, 60% to 80%, 70% to 80%, 10% to 70%, 20% to 70%, 30% to 70%, 40% to 70%, 50% to 70%, 60% to 70%, 10% to 60%, 20% to 60%, 30% to 60%, 40% to 60%, 50% to 60%, 10% to 50%, 20% to 50%, 30% to 50%, 40% to 50%, 10% to 40%, 20% to 40%, 30% to 40%, 10% to 30%, 20% to 30%, 10% to 20%, or any range or subrange formed by any of the aforementioned starting points and / or endpoints provided herein. The volume of the crystalline shell is approximately equal to the volume of the glass-ceramic article minus the volume of the amorphous interior. Thus, for example, if the amorphous interior occupies 60% of the volume of the glass-ceramic article, the crystalline shell will occupy approximately 40% of the volume of the glass-ceramic article.

[0098] In one or more embodiments, the depth D of the shell layer 110 of the glass ceramic article 100 may be at least 5 micrometers and at most 10 micrometers, at most 50 micrometers, at most 100 micrometers, at most 250 micrometers, at most 500 micrometers, at most 1 mm, at most 1.5 mm, or at most 2 mm. In one or more embodiments, the depth D of the shell layer 110 is at most half of the thickness T1 of the glass ceramic article 100.

[0099] The method for forming the glass ceramic product of the present disclosure may involve manufacturing a melt by forming the main component of the glass ceramic product, and then forming the composition into a glass product using various castings, drawing (such as slot drawing or fusion drawing), floating (such as on a molten tin bed) and bending processes. Once the glass product containing the components is formed, the surface of the glass product can be nucleated to promote crystal growth, thereby manufacturing the glass ceramic product. Crystal growth begins on the surface of the glass ceramic product and extends and extends into the glass ceramic product from then on. As described above, crystal growth can be oriented to be perpendicular to the surface of the glass ceramic product. In one or more embodiments, the crystal may or may not be completely vertical to the surface growth, such as, for example, the crystal can grow at an angle of less than or equal to 15 degrees with the normal of the surface. In one or more embodiments, crystal growth can stop when the crystal has been extended longitudinally to at least 5 microns. In addition, in one or more embodiments of manufacturing the glass ceramic product, crystal growth is stopped before extending to the center of the glass ceramic product to leave an amorphous interior in the glass ceramic product. However, according to one or more other embodiments of manufacturing the crystalline product, as described below, crystal growth can continue until the crystal meets at about the product center line. Crystal growth perpendicular to the surface is desirable because it improves transparency through crystals that are substantially parallel to the viewing plane, where the viewing plane is perpendicular to the surface of a given glass-ceramic article. Thus, the more perpendicular to the surface the crystal growth of each columnar crystal is, the better the transparency of the viewing plane.

[0100] Crystal nucleation may involve heat treatment of a glass article formed of a main component. Heat treatment may be performed in a furnace or any other suitable device to apply heat to the glass article to form a glass ceramic article. For certain example embodiments described in detail below, differential scanning calorimetry (DSC) is used to characterize the glass ceramic article for nucleation process. Differential scanning calorimetry (DSC) can measure the change in the difference in heat flow required to increase the temperature of a gram of sample and a reference material with temperature, which can be expressed as milliwatts per milligram (mW / mg) to degrees Celsius (°C). DSC is measured in a controlled atmosphere, where the measurement indicates changes involving endothermic and exothermic processes (such as exothermic processes of crystallization). The glass article is placed in a DSC instrument and the starting temperature (temperature at which melting / crystallization begins) and the peak temperature (temperature at which the mass heat flow of a given sample reaches the highest point) are collected by corresponding software measurements. In one or more embodiments, the exotherm onset temperature as measured by DSC is 1010°C to 1080°C, 1020°C to 1070°C, 1030°C to 1060°C, 1040°C to 1050°C, 1010°C to 1020°C, 1020°C to 1030°C, 1030°C to 1040°C, 1050°C to 1060°C, 1060°C to 1070°C, 1070°C to 1080°C, or any range or sub-range formed by any of the foregoing starting points and / or endpoints provided herein. In one or more embodiments, as measured by DSC, the exothermic peak temperature is 1060°C to 1130°C, 1070°C to 1120°C, 1080°C to 1110°C, 1080°C to 1100°C, 1060°C to 1070°C, 1070°C to 1080°C, 1080°C to 1090°C, 1090°C to 1100°C, 1100°C to 1110°C, 1110°C to 1120°C, or any range or sub-range formed by any of the foregoing starting points and / or endpoints provided herein. If the temperature at which the thermal treatment is performed is too low from the starting temperature, such as below 1010°C, nucleation may not begin. If the temperature at which the thermal treatment is performed is much higher than the exothermic peak temperature, such as above 1130°C, defects may form during the nucleation process.

[0101] During the heat treatment, the longer the heat treatment time of the glass-ceramic product is, the longer the nucleation process is carried out, which means that the shell thickness increases with the increase of the heat treatment time of the glass-ceramic product. Figures 5 to 8As shown, increasing the heat treatment time of the glass-ceramic article will increase the depth of the crystalline shell relative to the amorphous interior (wherein the shell is heat treated at 1050°C for 1 hour 3 minutes to 4 hours 36 minutes). In aspects of the present disclosure, the heat treatment can be carried out for greater than or equal to 1 hour and less than or equal to 5 hours. The heat treatment time required to achieve the desired amorphous interior thickness to shell thickness ratio can depend on the total thickness of the glass-ceramic article. Nevertheless, depending on the thickness of the glass-ceramic article and depending on the desired crystallinity, the heat treatment can be carried out for greater than 0 hours and less than 1 hour or greater than 5 hours.

[0102] Heat treatment of glass ceramic products to form a shell may produce surface textures, such as surface roughness, on the first major surface and / or second major surface of the glass ceramic product. Surface texture may reduce the transmittance through the glass, and reduce transparency. In one or more embodiments, such surface textures are removed from the glass ceramic product by polishing the glass ceramic product. Polishing can be any means to smooth the surface of the glass ceramic product or to reduce the surface texture by grinding the surface and / or thinning the surface of the glass ceramic product (even if slightly thinned). For glass ceramic products with planes, spherical surfaces and / or other surfaces, the glass ceramic product can be polished to produce a shape with a smooth surface (including but not limited to spherical, circular and / or flat). Since polishing occurs on the surface of the glass ceramic product, polishing may occur at least partially on the shell. Polishing glass products can be beneficial to improving transparency and preparing glass ceramic products for use in processes such as sealing and coating, making such processes easier to carry out on glass ceramic products.

[0103] To test the crack resistance of the shell, any of the numerous indentation tests can be performed on the shell, particularly after the surface has been polished to fully remove the surface texture. In one or more embodiments, the hardness test is a Vickers hardness test, during which an indentation is formed on the surface of the glass-ceramic article, from which the hardness and crack resistance of the crystalline shell can be determined. As will be discussed more comprehensively below, the crystals of the shell enhance crack resistance by forming a tortuous path for crack propagation. Under a preset kgf value, the Vickers hardness tester can be used to imprint the shell with a predetermined force, which is substantially sufficient to propagate cracks in the product embodiment. In one or more embodiments, during imprinting, the shell will show a tortuous crack path, which limits crack propagation and limits crack expansion. The tortuous path may be related to the vertical orientation of the columnar crystals of the shell relative to the surface of the glass-ceramic article.

[0104] like Figure 1BAs shown, the glass-ceramic article can exhibit high transparency, even embodiments where the crystals extend completely into the middle of the article, which will be discussed more fully below. In one or more embodiments, the glass-ceramic article is a sheet that is used as a transparent cover for a display device, such as an electronic device (e.g., a laptop screen, a tablet computer, a mobile device, etc.), an appliance (e.g., a stove top cover, an oven door, a refrigerator, a microwave oven, etc.), or a building panel (e.g., a window, a partition, etc.), etc.

[0105] When the glass ceramic article is viewed at an angle that is not substantially parallel to the crystal growth direction, the transparency may not be as high as when viewed along the parallel crystal growth direction. Therefore, in the present disclosure, the glass ceramic article application can be used for devices or building articles or structures that require privacy when the glass ceramic article is viewed at an angle that deviates from the normal to the surface of the glass ceramic article, such as flat-panel devices or windows.

[0106] Exemplary Embodiments

[0107] The glass composition that can effectively manufacture the glass-ceramic products described in this article is formed based on the mole % range of the components listed in Table 1. The labels 149AHI, 149AHJ and 149AHK each represent a glass-ceramic product composed of main components with different mole % ranges. The "batch mole %" in Table 1 represents the mole % range of each main component used in the glass-ceramic product according to the theoretical amount. The "analytical mole %" in Table 1 represents the mole % range of each main component used in the glass-ceramic product according to the actual amount. The data in Table 1 are rounded to the percentile, and the rounding assumed error causes 149AHI to have 0.01 mole % more and 149AHJ to have 0.01 mole % less.

[0108] Table 1: Composition and properties of the glass ceramic materials studied

[0109]

[0110] In a glass ceramic article formed of the 149AHI composition (also referred to as "149AHI" or "149AHI sample"), the glass ceramic article has a thickness of about 0.8 mm and a viscosity of 3.091 g / cm 3 (g / cm3) density. Figure 4 The graph shows how the DSC value changes with temperature when 149AHI is heat treated. Figure 4 The onset 100 of 149AHI shows a DSC exotherm onset temperature of about 1037°C, which is where the DSC value of 149AHI begins to increase rapidly. Figure 4 The peak 102 also illustrates that the DSC value of 149AHI reaches a maximum value at about 1087°C.

[0111] For 149AHI, the heat treatment occurred at 1050°C to promote nucleation at the surface of the article, where the shell of 149AHI became larger with increasing heat treatment time. Figures 5 to 8 Four points during the heat treatment were observed and recorded over time: 1 hour and 3 minutes ( Figure 5 )、2 hours and 33 minutes( Figure 6 )、3 hours 45 minutes( Figure 7 ) and 4 hours and 36 minutes ( Figure 8 ). Figures 5 to 8 As shown for 149AHI, the depth of the shells 200a, 200b, 200c, 200d increases as the heat treatment continues. The interiors 202a, 202b, and 202c show the amorphous interior of 149AHI decreasing. Over time, the shells become deeper and the crystals continue to grow substantially perpendicular to the surface. Figure 8 In the example, after 4 hours and 36 minutes of heat treatment, the shell grows to the extent that there is no amorphous interior, that is, the sample is completely crystallized.

[0112] similar Figures 5 to 7 , Fig. 9 The cross section of a glass-ceramic composite made from the 149AHI composition is shown when the glass-ceramic article is heat treated for 2 hours and 30 minutes to produce a glass-ceramic composite having a shell 206 with a depth of 130 microns from each surface. The total thickness of the glass-ceramic article is 0.8 mm, and the inner portion 204 is 540 microns.

[0113] The transmittance values ​​of 149AHI at different stages of heat treatment were recorded, including completely amorphous (ie, not yet heat treated), 130 micron shell thickness and 540 micron amorphous interior thickness, and completely crystalline (ie, no amorphous interior). Fig.10 The figure shows the total transmittance of 149AHI versus wavelength. Fig.10 As shown in curves 300 and 301 of FIG. 3 , the transmittance curve of the glass-ceramic article substantially overlaps with the curve of the fully amorphous glass, indicating that the composite material with a 130 micron shell layer exhibits high transparency comparable to the high transparency of a typical vitreous substrate. Fig.10 As shown in curve 302 of FIG. 3 , the fully crystalline form of 149AHI still exhibits relatively high transmittance and transparency in the visible light spectrum, wherein, for example, the fully crystalline form exhibits a total transmittance of about 75% for visible light with wavelengths as low as 500 nm. In addition, for light with wavelengths as low as about 375 nm, the fully crystalline form exhibits a total transmittance of over 60%. As will be discussed more fully below, applicants have discovered a way to improve the transparency of fully crystalline articles based on substantially reducing or eliminating secondary phases during crystal nucleation and growth.

[0114] The visibility of a particular transmittance may be very subjective to the viewer, but generally speaking, a transmittance in the visible light spectrum of more than 30% can be considered as reasonable transparency for some applications. For most applications, a transmittance of 50% or 60% provides sufficient transparency. Therefore, a glass-ceramic article with a transmittance of more than 80% (including to wavelengths as low as about 380nm) of 149AHI can be expected to be suitable for display applications.

[0115] Fig.11 and Fig.12 The fully crystalline form of 149AHI shown in FIG. 1 has a very low axial transmittance in the visible light spectrum. For example, Fig.11 Point 304 indicates that the axial transmittance for light of wavelength 500 nm is only about 20%. Fig.12 Point 306 indicates that the diffuse transmittance in the visible light spectrum is quite high, including nearly 60% at 500nm. In contrast, the glass-ceramic version of 149AHI behaves similarly to the fully amorphous version of 149AHI in terms of axial transmittance (transmittance in the visible spectrum range>80%) and diffuse transmittance (transmittance in the visible spectrum range<10%).

[0116] Fig.13 The scattering ratios of the fully amorphous, fully crystalline, and glass-ceramic forms of 149AHI are plotted. The scattering ratios of the fully crystalline form in the visible light spectrum (see Fig.13 The curve 308 of Figure 308 is significantly higher than that of amorphous and glass-ceramic types. Compared with amorphous glass, which has almost no light scattering in the visible light spectrum (thus, the scattering ratio of the completely amorphous type in the visible light spectrum is nearly 0% [see Fig.13 The crystals in the shell promote greater light scattering in the visible light spectrum for the fully crystalline form. The scattering ratio of the glass-ceramic form is well below 20%, and even below 10% in most of the visible spectrum.

[0117] Fig.14 The X-ray diffraction intensity versus 2θ for a fully crystalline 149AHI sample is shown (i.e., after heat treatment at 1050°C for 4 hours and 36 minutes, the surface crystals of the 149AHI sample grown in the central phase will form a fully crystalline form, leaving very little (if any) amorphous content). It is assumed that an amorphous or glassy structure will have a more consistent curve than Fig.14 The fully crystalline form has a diffraction pattern that is highly representative of a crystalline structure, as seen by the clear large peak along the 2θ axis. In addition, the diffraction pattern matches Sr(Al2Si2O8) very well, although as will be discussed below, based on the thickness of the fully crystalline sample analyzed, a secondary crystalline phase may also be present.

[0118] The crack paths of embodiments of glass-ceramic articles are examined to understand the crack resistance of the articles. Fig.15The Vickers indentation of the fully crystalline form of the AHI of FIG149 is shown. Prior to indentation, the surface was polished to remove 100 microns from the surface, eliminating any surface texture formed during the heat treatment. In the exemplary embodiment described in this paragraph, the shell layer is about 421.61 microns thick (this is Figure 8 of the combined shell divided by 2, minus 100 microns of polishing). Fig.15 The crack 400 shows that the crack caused by the stamping follows a tortuous path. As described herein, a tortuous crack path can reduce the propagation of cracks in a glass ceramic article more than a straight crack. Fig.15 It can be seen that the zigzag crack 400 is at least partially caused by the growth of columnar crystals extending from the surface of the glass-ceramic article.

[0119] Likewise, Fig.16 Shown is a Vickers indent applied to 149AHI, a glass-ceramic composite that was heat treated for 2 hours and 30 minutes and polished to produce a 130 micron shell and 540 micron amorphous interior. Fig.15 , Fig.16 The composite material has a tortuous crack path (see Fig.16 The cracking 402) indicates that the shell of the glass-ceramic composite material has greater crack resistance than the amorphous glass of the same composition.

[0120] In addition to composite glass-ceramic articles having an amorphous interior and a crystalline shell, applicants have discovered that fully crystalline forms are also suitable for use as transparent displays. Specifically, the transparency of fully crystalline articles can be improved by maintaining the SiO2-Al2O3-SrO glass composition within slightly narrow limits and by limiting the article thickness to 1 mm or less. More specifically, the crystalline article is essentially a single crystal phase, particularly Sr(Al2Si2O8), and forms extremely fine secondary crystalline phases, such as SrSiO3, which reduces transparency and reduces mechanical reliability. As will be discussed more fully below, the crystalline article is manufactured by nucleating columnar crystals from the surface of the glass article until the columnar crystals meet at approximately the midpoint of the thickness of the glass article.

[0121] Fig.17 The evolutionary stages of the crystalline article 200 are depicted, which substantially correspond to the above discussion. In the first stage 202, an amorphous glass article 204 is provided. As described above and discussed more fully below, the amorphous glass article 204 primarily comprises silicon oxide (SiO2), aluminum oxide (Al2O3), and strontium oxide (SrO). The amorphous glass article 204 includes a first major surface 206 and a second major surface 208. The second major surface 208 is opposite to the first major surface 206, and the distance between the first major surface 206 and the second major surface 208 defines the thickness T of the amorphous glass article 204. A minor surface 210 connects the first major surface 206 and the second major surface 208.

[0122] As shown in the second stage 212, the amorphous glass article 204 is heat treated to nucleate the crystallized regions 214, 216 (similar to the shell 110 described above) on the first major surface 206 and the second major surface 208, respectively. In one or more embodiments, the crystallized regions 214, 216 are formed by heterogeneous nucleation without a nucleating agent. In other words, and more specifically, the crystallized regions 214, 216 are surface nucleated, for example, from defects on the first major surface 206, the second major surface 208, and the secondary surface 210 to promote inward crystal growth to form columnar crystals 218. Although not specifically shown in FIG. Fig.17 , a crystalline region is also formed on the secondary surface 210. The crystalline regions 214, 216 are defined by columnar crystals 218 extending from the respective first major surface 206 and the second major surface 208 into the depth of the amorphous region 220. The formation of the crystalline regions 214, 216 transforms the amorphous glass article 204 into a glass ceramic article 222.

[0123] Consistent with the above, the crystals 218 are described as "columnar" meaning that the crystals have a high aspect ratio (height to width), such as at least 2:1, at least 10:1, at least 20:1, or at least 50:1, and are substantially oriented perpendicular to the respective first major surface 206 and the second major surface 208, for example within 15 degrees of the normal. As described above, the columnar crystals 218 are oriented perpendicularly or nearly perpendicularly in the crystalline regions 214, 216 to create a relatively high transparency and improved radial crack resistance for the crystalline regions 214, 216, compared to randomly oriented crystals (which can be generated in the glass-ceramic article 222 via heterogeneous nucleation using a nucleating agent and / or via homogeneous nucleation).

[0124] As the glass-ceramic article 222 continues to be heat treated, the crystalline regions 214, 216 continue to grow deep into the amorphous region 220, thereby shrinking the amorphous region 220, as shown in the third stage 224. As the heat treatment continues, as shown in the fourth stage 226, the crystalline regions 214, 216 continue to grow until they meet to produce a crystalline article 200. Fig.17 As can be seen, the amorphous region 220 is substantially, if not completely, removed from the crystalline article 200. In this manner, the crystalline regions 214, 216 nucleate and grow at the respective first and second major surfaces 206, 208 until they meet at approximately the midline of the thickness T.

[0125] In one or more embodiments, each of the crystalline regions 214, 216 is at least 90 volume % crystalline phase, at least 92 volume % crystalline phase, at least 94 volume % crystalline phase, at least 96 volume % crystalline phase, at least 98 volume % crystalline phase, or greater than 99 volume % crystalline phase. In one or more embodiments, each of the crystalline regions 214, 216 comprises 100 volume % crystalline phase. Additionally, in one or more embodiments, the crystalline article 200 is overall at least 90 volume % crystalline phase, at least 92 volume % crystalline phase, at least 94 volume % crystalline phase, at least 96 volume % crystalline phase, at least 98 volume % crystalline phase, or greater than 99 volume % crystalline phase. In one or more embodiments, the crystalline article 200 overall comprises 100 volume % crystalline phase. In one or more embodiments, the crystalline article 200 is overall 10 volume % or less amorphous phase, 8 volume % or less amorphous phase, 6 volume % or less amorphous phase, 4 volume % or less amorphous phase, 2 volume % or less amorphous phase, or 1 volume % or less amorphous phase. In one or more embodiments, the crystalline article 200 does not contain an amorphous phase.

[0126] As described above, the crystalline article mainly comprises silica, alumina, and strontium oxide (collectively referred to as the "main components"). In one or more embodiments, the main components account for at least 85 mol % of the crystalline article 200, at least 87.5 mol % of the crystalline article 200, at least 90 mol % of the crystalline article 200, at least 92.5 mol % of the crystalline article 200, at least 95 mol % of the crystalline article 200, at least 97.5 mol % of the crystalline article 200, or up to 100 mol % of the crystalline article 200. In one or more embodiments, the crystalline article 200 comprises an amount of the main components of 85 mol % to 100 mol %, 87.5 mol % to 100 mol %, 90 mol % to 100 mol %, 92.5 mol % to 100 mol %, 95 mol % to 100 mol %, 97.5 mol % to 100 mol %, or any range or sub - range therebetween bounded by the foregoing endpoints.

[0127] As described above, the crystalline article 200 can be formed from a glass composition that can be regarded as a subset of a broader composition suitable for forming a glass - ceramic article having an amorphous interior. In one or more embodiments, the composition of the crystalline article includes 40 mol % to 50 mol % silica (SiO2), with the alumina (Al2O3) inventory being more than the strontium oxide (SrO) by up to 5 mol %, i.e., 0 mol % < Al2O3–SiO2 ≤ 5 mol %.

[0128] In one or more embodiments, the crystalline article 200 may include an amount of silicon oxide (SiO2) in the following ranges: 40 mol% ≤ silicon oxide ≤ 50 mol%, 41 mol% ≤ silicon oxide ≤ 50 mol%, 42 mol% ≤ silicon oxide ≤ 50 mol%, 43 mol% ≤ silicon oxide ≤ 50 mol%, 44 mol% ≤ silicon oxide ≤ 50 mol%, 45 mol% ≤ silicon oxide ≤ 50 mol%, 46 mol% ≤ silicon oxide ≤ 50 mol%, 47 mol% ≤ silicon oxide ≤ 50 mol%, 48 mol% ≤ silicon oxide ≤ 50 mol%, 49 mol% ≤ silicon oxide ≤ 50 mol%, 40 mol% ≤ silicon oxide ≤ 49 mol%, 41 mol% ≤ silicon oxide ≤ 49 mol%, 42 mol% ≤ silicon oxide % ≤ 49 mol% silicon oxide, 43 mol% ≤ 49 mol% silicon oxide, 44 mol% ≤ 49 mol% silicon oxide, 45 mol% ≤ 49 mol% silicon oxide, 46 mol% ≤ 49 mol% silicon oxide, 47 mol% ≤ 49 mol% silicon oxide, 48 mol% ≤ 49 mol% silicon oxide, 40 mol% ≤ 48 mol% silicon oxide, 41 mol% ≤ 48 mol% silicon oxide, 42 mol% ≤ 48 mol% silicon oxide, 43 mol% ≤ 48 mol% silicon oxide, 44 mol% ≤ 48 mol% silicon oxide, 45 mol% ≤ 48 mol% silicon oxide, 46 mol% ≤ 48 mol% silicon oxide, 47 mol% ≤ 48 ... %≤silicon oxide≤47 mol%, 41 mol%≤silicon oxide≤47 mol%, 42 mol%≤silicon oxide≤47 mol%, 43 mol%≤silicon oxide≤47 mol%, 44 mol%≤silicon oxide≤47 mol%, 45 mol%≤silicon oxide≤47 mol%, 46 mol%≤silicon oxide≤47 mol%, 40 mol%≤silicon oxide≤46 mol%, 41 mol%≤silicon oxide≤46 mol%, 42 mol%≤silicon oxide≤46 mol%, 43 mol%≤silicon oxide≤46 mol%, 44 mol%≤silicon oxide≤46 mol%, 45 mol%≤silicon oxide≤46 mol%, 40 mol%≤silicon oxide≤45 mol%, 41 mol%≤silicon oxide≤45 mol%, 4 %≤silicon oxide≤45 mol%, 43 mol%≤silicon oxide≤45 mol%, 44 mol%≤silicon oxide≤45 mol%, 40 mol%≤silicon oxide≤44 mol%, 41 mol%≤silicon oxide≤44 mol%, 42 mol%≤silicon oxide≤44 mol%, 43 mol%≤silicon oxide≤44 mol%, 40 mol%≤silicon oxide≤43 mol%, 41 mol%≤silicon oxide≤43 mol%, 42 mol%≤silicon oxide≤43 mol%, 40 mol%≤silicon oxide≤42 mol%, 41 mol%≤silicon oxide≤42 mol%, 40 mol%≤silicon oxide≤41 mol%, and any range or sub-range formed by any of the foregoing starting points and / or endpoints provided herein.

[0129] In aspects of the present disclosure, the crystalline article 200 may include an amount of aluminum oxide (Al2O3) of 25 mol% ≤ alumina ≤ 32.5 mol%, such as 26 mol% ≤ alumina ≤ 32.5 mol%, 27 mol% ≤ alumina ≤ 32.5 mol%, 28 mol% ≤ alumina ≤ 32.5 mol%, 29 mol% ≤ alumina ≤ 32.5 mol%, 30 mol% ≤ alumina ≤ 32.5 mol%, 31 mol% ≤ alumina ≤ 32.5 mol%, 32 mol% ≤ alumina ≤ 32.5 mol%, 25 mol% ≤ alumina ≤ 31 mol%, 26 mol% ≤ alumina ≤ 31 mol%, 27 mol% ≤ alumina ≤ 31 mol%, 28 mol% ≤ alumina ≤ 31 mol%, 29 mol% ≤ alumina ≤ 31 mol%, 30 mol% ≤ alumina ≤ 31 mol%, %, 25 mol % ≤ alumina ≤ 30 mol %, 26 mol % ≤ alumina ≤ 30 mol %, 27 mol % ≤ alumina ≤ 30 mol %, 28 mol % ≤ alumina ≤ 30 mol %, 29 mol % ≤ alumina ≤ 30 mol %, 25 mol % ≤ alumina ≤ 29 mol %, 26 mol % ≤ alumina ≤ 29 mol %, 27 mol % ≤ alumina ≤ 29 mol %, 28 mol % ≤ alumina ≤ 29 mol %, 25 mol % ≤ alumina ≤ 28 mol %, 26 mol % ≤ alumina ≤ 28 mol %, 27 mol % ≤ alumina ≤ 28 mol %, 25 mol % ≤ alumina ≤ 27 mol %, 26 mol % ≤ alumina ≤ 27 mol %, 25 mol % ≤ alumina ≤ 26 mol %, or any range or sub-range formed by any of the foregoing starting points and / or endpoints provided herein.

[0130] In aspects of the present disclosure, the crystalline article 200 may include an amount of strontium oxide (SrO) of 22.5 mol % ≤ strontium oxide ≤ 30 mol %, such as 23 mol % ≤ strontium oxide ≤ 30 mol %, 24 mol % ≤ strontium oxide ≤ 30 mol %, 25 mol % ≤ strontium oxide ≤ 30 mol %, 26 mol % ≤ strontium oxide ≤ 30 mol %, 27 mol % ≤ strontium oxide ≤ 30 mol %, 28 mol % ≤ strontium oxide ≤ 30 mol %, 29 mol % ≤ strontium oxide ≤ 30 mol %, 22.5 mol%≤strontium oxide≤29 mol%, 23 mol%≤strontium oxide≤29 mol%, 24 mol%≤strontium oxide≤29 mol%, 25 mol%≤strontium oxide≤29 mol%, 26 mol%≤strontium oxide≤29 mol%, 27 mol%≤strontium oxide≤29 mol%, 28 mol%≤strontium oxide≤29 mol%, 22.5 mol%≤strontium oxide≤28 mol%, 23 mol%≤strontium oxide≤28 mol%, 24 mol%≤strontium oxide≤28 mol% , 25 mol% ≤ strontium oxide ≤ 28 mol%, 26 mol% ≤ strontium oxide ≤ 28 mol%, 27 mol% ≤ strontium oxide ≤ 28 mol%, 22.5 mol% ≤ strontium oxide ≤ 27 mol%, 23 mol% ≤ strontium oxide ≤ 27 mol%, 24 mol% ≤ strontium oxide ≤ 27 mol%, 25 mol% ≤ strontium oxide ≤ 27 mol%, 26 mol% ≤ strontium oxide ≤ 27 mol%, 22.5 mol% ≤ strontium oxide ≤ 26 mol%, 23 mol% ≤ strontium oxide ≤ 26 mol %≤strontium oxide≤26 mol%, 25 mol%≤strontium oxide≤26 mol%, 22.5 mol%≤strontium oxide≤25 mol%, 23 mol%≤strontium oxide≤25 mol%, 24 mol%≤strontium oxide≤25 mol%, 22.5 mol%≤strontium oxide≤24 mol%, 23 mol%≤strontium oxide≤24 mol%, 22.5 mol%≤strontium oxide≤23 mol%, or any subrange formed by any of the foregoing starting points and / or endpoints provided herein.

[0131] Consistent with the above, the composition used to form the crystalline article 200 may further include a minor component, which is a component that is present in the glass ceramic article individually in an amount of 1 mol % or less, 0.5 mol % or less, 0.2 mol % or less, 0.1 mol % or less, or 0.05 mol % or less. The total amount of the minor components (all minor components added together) may be present in the crystalline article 200 in an amount of 5 mol % or less, 2 mol % or less, 1 mol % or less, 0.5 mol % or less, 0.2 mol % or less, or 0.1 mol % or less. In aspects of the present disclosure, the minor component may be magnesium oxide, calcium oxide, barium oxide, sodium oxide, potassium oxide, iron oxide, and / or titanium oxide, etc. In one or more embodiments, the composition of the crystalline glass ceramic article 200 may contain up to 5 mol % of boron oxide (BO), such as about 1 mol % to 5 mol %, without affecting the expected properties of the crystalline article 200.

[0132] The method of forming the crystalline article 200 of the present disclosure is substantially the same as that described above with respect to the related glass-ceramic article. However, the heat treatment is continued until the crystallized regions 214, 216 meet at substantially the midline of the thickness of the crystalline article 200. After the heat treatment, the first major surface and / or the second major surface of the crystalline article 200 may be polished to remove surface texture and increase transmittance, as described above.

[0133] although Fig.17 A substantially planar (e.g., sheet-like) crystalline article 200 is depicted, but the crystalline article 200 may still be formed according to a certain size range and shape. In one or more other embodiments, the crystalline article 200 may be a rectangular article. In one or more embodiments, the crystalline article 200 may be a spherical article, such as a sphere or an ellipsoid. In yet one or more other embodiments, the crystalline article 200 may have a combination of a sphere and a plane, such as a hemisphere. The applications in which the crystalline article can be used are the same as those of the related glass-ceramic articles described above.

[0134] Fig.18 A SEM micrograph depicting the interface between the crystalline regions 214, 216 of the crystalline article 200 having a thickness of 0.53 mm. A 149AHI composition was used to form the crystalline article 200. To form the crystalline regions 214, 216, the amorphous glass was maintained at 1070°C for 133 minutes.

[0135] Fig.19 Depicted is a SEM micrograph of a crystalline article 200 having a thickness of 1.00 mm, wherein crystalline regions 214, 216 are produced by maintaining an amorphous glass at 1070°C for 250 minutes. Fig. 20 Depicted is a SEM micrograph of a crystalline article 200 having a thickness of 1.03 mm, wherein crystalline regions 214, 216 are produced by maintaining an amorphous glass at 1060°C for 330 minutes. Fig.21 Depicted is a SEM micrograph of a crystalline article 200 having a thickness of 1.17 mm, wherein crystalline regions 214, 216 are produced by maintaining an amorphous glass at 1070°C for 300 minutes. Figures 19 to 21 The crystalline product 200 is composed of Fig.17 The glass composition of the crystalline product 200 is prepared. Figures 17 to 21 It can be seen that the crystalline phase of the crystalline product changes as the thickness of the glass-ceramic product increases.

[0136] Specifically, Fig.18 The crystalline glass-ceramic products consist of a single structure of crystalline material (gray area in the SEM micrograph), while Figures 19 to 21 The crystalline product comprises at least two structures of crystalline material (gray area and white area in the SEM micrograph). Fig. 22 and Fig.23 As shown, Fig.18 and Fig.21 Energy dispersive spectroscopy (EDS) was performed on the crystalline samples to determine the characteristics of each crystalline structure.

[0137] Fig. 22 The gray areas within the SEM micrographs of the 0.53 mm samples shown have substantially the same elemental composition. That is, the peaks for the various detected elements (O, Al, Si, Sr) have substantially the same intensity, indicating that the crystals have substantially the same composition. In contrast, Fig.23 The figure shows that the Sr content is enriched in the white phase relative to the Sr content in the gray phase. Therefore, the Sr content in the white phase is greater than that in the gray phase.

[0138] To determine the actual composition of each phase, powder X-ray diffraction (XRD) was performed on fully crystalline samples made from the 149AHI composition (heat treated for the same time, 4 hours and 34 minutes). One sample had a thickness of 0.52 mm and the other had a thickness of 1.07 mm. Fig.24 The XRD spectrum of the sample with a thickness of 0.52 mm is plotted. Fig.24 It can be seen that the peak of the spectrum is consistent with the Sr(Al2Si2O8) single crystal (as shown by the vertical line extending from the x-axis). Fig.25 The XRD spectrum of the sample with a thickness of 1.07 mm is plotted. Fig.25 It can be seen that the peak of the spectrum corresponds not only to the Sr(Al2Si2O8) crystalline phase, but also to the SrSiO3 crystalline phase (as shown by the vertical line extending from the x-axis). Therefore, using the same composition and heat treatment to produce crystalline products with different crystalline phases allows the applicant to infer that the thickness difference is the main cause of the growth of the secondary phase.

[0139] Using image analysis, determine the presence of Figures 19 to 21 The amount of secondary phase (SrSiO3) in each crystalline glass-ceramic is provided in Table 2.

[0140] Table 2: Secondary crystalline phase amount based on sample thickness

[0141] Sample thickness Area percentage of secondary phase 1.00mm 4.74% 1.03mm 7.42% 1.17mm 8.44%

[0142] From Table 2, it can be seen that the amount of secondary crystalline phase increases with the thickness of the crystalline product. Fig.18 In a crystalline article having a thickness of 100 μm, applicants speculate, without wishing to be bound by theory, that secondary phase formation may be inhibited based on the thickness of the crystalline article. Specifically, it is hypothesized that as the crystal grows, crystal formation pushes unconsumed elements into the remaining glass phase, ultimately resulting in an enriched composition that is susceptible to crystallization of a new phase. Thicker crystalline articles start with larger amorphous sections that are enriched in unconsumed elements, thereby more readily creating conditions that allow secondary phases to form.

[0143] Thus, in one or more embodiments, the thickness T of the crystalline article 200 is 1 mm or less, in particular 0.95 mm or less, 0.9 mm or less, 0.85 mm or less, 0.8 mm or less, 0.75 mm or less, 0.7 mm or less, 0.65 mm or less, 0.6 mm or less, 0.55 mm or less, 0.5 mm or less, 0.45 mm or less, 0.4 mm or less, 0.35 mm or less, 0.3 mm or less, 0.25 mm or less, 0.2 mm or less, 0.15 mm or less, 0.1 mm or less. In one or more embodiments, the thickness T of the crystalline article 200 is 0.05 mm or more, 0.1 mm or more, 0.15 mm or more, 0.2 mm or more, 0.25 mm or more, 0.3 mm or more, 0.35 mm or more, 0.4 mm or more, 0.45 mm or more, or 0.5 mm or more. In one or more embodiments, the thickness T of the crystalline article 200 is 0.05 mm to 1 mm, 0.1 mm to 1 mm, 0.15 mm to 1 mm, 0.2 mm to 1 mm, 0.25 mm to 1 mm, 0.3 mm to 1 mm, 0.35 mm to 1 mm, 0.4 mm to 1 mm, 0.45 mm to 1 mm, or 0.5 mm to 1 mm.

[0144] In one or more embodiments, the crystalline product 200 comprises at least 90% by volume of a single crystalline phase (particularly having a Sr(Al2Si2O8) structure), at least 91% by volume of a single crystalline phase, at least 92% by volume of a single crystalline phase, at least 93% by volume of a single crystalline phase, at least 94% by volume of a single crystalline phase, at least 95% by volume of a single crystalline phase, at least 96% by volume of a single crystalline phase, at least 97% by volume of a single crystalline phase, at least 98% by volume of a single crystalline phase, or at least 99% by volume of a single crystalline phase. In one or more embodiments, the crystalline product 200 comprises no more than 10% by volume of a secondary crystalline phase (particularly having a SrSiO3 structure), no more than 9% by volume of a secondary crystalline phase, no more than 8% by volume of a secondary crystalline phase, no more than 7% by volume of a secondary crystalline phase, no more than 6% by volume of a secondary crystalline phase, no more than 5% by volume of a secondary crystalline phase, no more than 4% by volume of a secondary crystalline phase, no more than 3% by volume of a secondary crystalline phase, no more than 2% by volume of a secondary crystalline phase, or no more than 1% by volume of a secondary crystalline phase.

[0145] Providing a crystalline article 200 having a single crystalline phase material, particularly columnar crystals of such material, can increase the transmittance of light in the visible spectrum through the crystalline article 200 . Fig.26Transmission through a crystalline article 200 is plotted for articles having thicknesses of 0.40 mm, 0.87 mm, and 1.0 mm. Crystalline article 200 is formed from a 149AHI composition. The 0.40 mm sample was heat treated at 1070°C for 2 hours and 13 minutes. The 0.87 mm sample was heat treated at 1070°C for 4 hours and 10 minutes, and the 1.0 mm sample was heat treated at 1070°C for 5 hours. Each sample was fully crystalline (i.e., the surface nucleated crystalline regions 214, 216 met at approximately the midline of each sample). Fig.26 As can be seen, samples with a thickness of less than 1 mm have a transmittance of over 70% in the visible spectrum. In fact, samples with thicknesses of 0.40 mm and 0.87 mm have a transmittance of about 80% or more in the visible spectrum, with the 0.40 mm thick sample having a transmittance of nearly 90%. In contrast, the transmittance of the 1 mm thick sample in the visible spectrum is greatly reduced, being less than 60% for most of the visible spectrum and less than 70% for the entire visible spectrum. Again, while it is expected that the transmittance will decrease slightly with increasing sample thickness, it is believed that the sharp decrease in transmittance is related to the formation of secondary crystalline phases, which are more abundant in thick samples.

[0146] Fig. 27 This supports the inference that the existence of the secondary crystalline phase leads to a decrease in transmittance. Fig. 27 The transmittance of a 0.40 mm thick sample containing a single crystalline phase (i.e., Sr(Al2Si2O8)) is plotted, and as described, the transmittance is nearly 90% for most (if not all) of the visible spectrum. The curve immediately below the 0.40 mm thick sample represents the calculated transmittance of a 1.0 mm (normalized) sample containing only a single crystalline phase of Sr(Al2Si2O8). As can be seen from the figure, the transmittance varies very little with thickness, where the structure is still a single crystalline phase. However, the next lower curve depicts the transmittance of an actual 1.0 mm sample made of the same composition as the 0.40 mm thick sample, which contains a secondary crystalline phase. As can be seen from the curve, the transmittance drops sharply, which applicant attributes to the presence of the secondary crystalline phase.

[0147] To test the crack resistance of the crystallized article, a Vickers hardness test was performed, during which an indentation was formed on the surface of the crystallized article, from which the hardness and crack resistance of the crystallized article could be determined. Consistent with the above findings, it was observed that columnar crystals enhance crack resistance by forming a tortuous path for crack propagation. Fig.28 The Vickers indentation on a crystalline article of the 149AHI composition is shown. Prior to indentation, the surface was polished to remove 100 microns from the surface, eliminating any surface texture formed during heat treatment. In the exemplary embodiment described in this paragraph, the crystalline article was about 0.4 mm thick. Subsequently, the Vickers indenter was loaded with 1 kgf, causing cracks to form in the crystalline article. Fig.28As shown, cracking follows a tortuous path, at least in part caused by columnar crystal growth extending from the surface of the crystalline article.

[0148] Fig.29 and Fig.30 Another embodiment of a crystalline article 200 is depicted. The crystalline article is formed from a glass composition nominally comprising 40 mol % SiO2, 32.5 mol % Al2O3, and 27.5 mol % SrO ("177EEF composition"), the glass composition being cast at a thickness of 0.52 mm. The glass composition is maintained at 1070°C to nucleate crystal formations, and the glass composition is maintained at that temperature for 2 hours and 52 minutes, thereby forming Fig.30 The fully crystalline product shown. Fig.30 The formation of columnar crystals can be clearly seen, but the interface between the first and second crystalline regions at the midpoint of the thickness is not as obvious as that of other samples (for example, compared to Figure 8 from Fig.29 It can be seen that the crystalline product 200 formed of the 177EEF composition is substantially transparent (ie, the text below the crystalline product 200 is clearly visible).

[0149] While experimenting with different compositions, the applicant discovered that compositions containing 40 to 50 mol% silicon oxide and aluminum oxide (equal to or up to 5 mol% more than strontium oxide) maintained favorable mechanical properties and acceptable transparency. Samples containing excess strontium oxide relative to aluminum oxide tend to form more secondary phases (SrSiO3), which reduces transparency and reduces mechanical reliability. Therefore, in one or more embodiments, strontium oxide is maintained less than aluminum oxide. However, a significant excess of aluminum oxide relative to strontium oxide can also produce poor optical transparency and poor mechanical reliability. Therefore, in one or more embodiments, aluminum oxide does not exceed 5 mol% more than strontium oxide.

[0150] The construction and arrangement of the components, components and structures as shown in various exemplary embodiments are only illustrative. Although only a few embodiments are described in detail herein, many modifications can be made (e.g., changing the size, dimensions, structure, shape and proportion, parameter values, installation arrangements, material use, color, orientation of various components) without substantially departing from the novel teachings and advantages of the subject matter described herein. The materials described herein can be used for purposes other than cover glass or window glass, such as for household goods, decorations, tableware, optical technology, etc. The order or sequence of any process, logical algorithm or method steps can be changed or reordered according to alternative embodiments and / or aspects. Without departing from the scope of the present invention, other replacements, modifications, changes and omissions can also be made to the design, operating conditions and arrangements of the aspects in the present disclosure.

Claims

1. A glass ceramic product comprising: 25 mol%≤silicon oxide≤60 mol%; 12.5 mol % ≤ alumina ≤ 45 mol %; and 12.5 mol% ≤ strontium oxide ≤ 45 mol%; wherein the interior of the glass-ceramic product is mostly amorphous glass; and The interior portion is at least partially surrounded by a mostly crystalline shell, the shell defining a first major surface on a first side of the interior portion and a second major surface on a second side of the interior portion opposite the first major surface.

2. The glass-ceramic article of claim 1, wherein the shell layer extends from one or both of the first major surface and the second major surface to a depth greater than or equal to 5 microns.

3. A glass-ceramic article as described in claim 1 or claim 2, wherein the shell layer comprises crystals, wherein a majority of the crystals are formed to be within 15 degrees of a normal line to one or both of the first major surface and the second major surface of the glass-ceramic article.

4. The glass-ceramic article of any one of claims 1 to 3, wherein the volume of the shell layer is less than 50% of the volume of the glass-ceramic article.

5. The glass-ceramic article according to any one of claims 1 to 4, wherein an absolute value of a difference between the first thermal expansion coefficient of the inner portion and the second thermal expansion coefficient of the shell layer is not greater than 2 μm / (m°C).

6. The glass-ceramic article of any one of claims 1 to 5, wherein the shell layer comprises crystals of SrAl2Si2O8.

7. The glass-ceramic article of any one of claims 1 to 6, wherein the aluminum oxide is present in an amount within 1 mol % of the amount of strontium oxide.

8. The glass-ceramic article of any one of claims 1 to 7, wherein the interior is at least 99% amorphous by volume and the shell is at least 99% crystalline by volume.

9. The glass-ceramic article of claim 8, wherein the transition between the shell and the interior is abrupt such that the glass-ceramic article changes from at least 99% crystalline by volume to at least 99% amorphous by volume in a distance of less than 10 microns.

10. The glass-ceramic article of any one of claims 1 to 9, comprising 1 mol % or less of other ingredients individually and 5 mol % or less of all other ingredients in total.

11. A glass-ceramic article as described in any one of claims 1 to 10, wherein at least 80% of light having a wavelength in the range of 400nm to 800nm ​​incident on one of the first major surface or the second major surface of the glass-ceramic article is axially transmitted through the glass-ceramic article to the other of the first major surface or the second major surface.

12. A glass ceramic product comprising: a first crystalline shell extending from a first major surface of the glass-ceramic article toward a centerline of the glass-ceramic article to a first depth; a second crystalline shell extending to a second depth from a second major surface of the glass-ceramic article toward the centerline, the second major surface being opposite the first major surface and the centerline being midway between the first major surface and the second major surface; and an amorphous interior, disposed between the first crystalline shell layer and the second crystalline shell layer; wherein the first crystalline shell layer and the second crystalline shell layer comprise a first coefficient of thermal expansion (CTE), and the amorphous interior comprises a second CTE; The absolute value of the difference between the first CTE and the second CTE is 2 μm / (m° C.).

13. The glass-ceramic article of claim 12, wherein each of the first crystalline shell layer, the second crystalline shell layer, and the amorphous interior layer comprises the same composition.

14. The glass-ceramic article of claim 13, wherein the composition comprises silicon oxide, aluminum oxide, and strontium oxide.

15. The glass-ceramic article of claim 14, wherein the composition comprises 25 mol%≤silicon oxide≤60 mol%; 12.5 mol%≤aluminum oxide≤45 mol%; and 12.5 mol%≤strontium oxide≤45 mol%.

16. The glass-ceramic article of any one of claims 12 to 15, wherein the first depth is 5 microns to 250 microns, and wherein the second depth is 5 microns to 250 microns.

17. The glass-ceramic article of claim 16, wherein the first depth is approximately equal to the second depth.

18. The glass-ceramic article of any one of claims 12 to 17, wherein each of the first crystalline shell layer and the second crystalline shell layer comprises columnar crystals extending from the first major surface and the second major surface, respectively.

19. The glass-ceramic article of claim 18, wherein the columnar crystals are within 15 degrees of a normal to each of the first and second major surfaces.

20. The glass-ceramic article of any one of claims 12 to 19, wherein the transition between at least one of the first crystalline shell or the second crystalline shell and the amorphous interior is abrupt such that the glass-ceramic article changes from being at least 99% crystalline by volume in the first crystalline shell or the second crystalline shell to being at least 99% amorphous by volume in the amorphous interior within a distance of less than 10 microns.

21. A glass-ceramic article as described in any one of claims 12 to 20, wherein at least 80% of light having a wavelength in the range of 400 nm to 800 nm incident on one of the first major surface or the second major surface of the glass-ceramic article is axially transmitted through the glass-ceramic article to the other of the first major surface or the second major surface.

22. A method for manufacturing a glass ceramic product, comprising: Columnar crystals are nucleated at a surface of the glass article to form a crystalline shell around an amorphous interior, the columnar crystals extending to a depth of at least 5 microns into the glass-ceramic article.

23. The method of claim 22, wherein nucleating comprises heat treating the glass article at a temperature in the range of 1010°C to 1080°C.

24. The method of claim 23, wherein the heat treatment is performed for a period of 1 hour to 5 hours.

25. The method of claim 23 or claim 24, further comprising polishing the surface by grinding a portion of the crystallized crust after heat treating.

26. The method according to any one of claims 22 to 25, wherein the depth of the crystalline shell is up to 250 micrometers.

27. The method according to any one of claims 22 to 26, wherein prior to nucleation, the method further comprises forming the glass article from a glass composition comprising 25 mol% ≤ silica ≤ 60 mol%; 12.5 mol% ≤ alumina ≤ 45 mol%; and 12.5 mol% ≤ strontium oxide ≤ 45 mol%.

28. The method according to any one of claims 22 to 27, wherein the crystalline shell comprises a first coefficient of thermal expansion (CTE), and the amorphous interior comprises a second CTE, wherein the absolute value of the difference between the first CTE and the second CTE is 2 μm / (m·°C).

29. The method according to any one of claims 22 to 28, wherein the columnar crystals are within 15 degrees of a line orthogonal to the surface.

30. The method according to any one of claims 22 to 29, wherein the transition between the crystalline shell and the amorphous interior is abrupt such that the glass-ceramic article changes from being at least 99% crystalline by volume in the crystalline shell to being at least 99% amorphous by volume in the amorphous interior over a distance of less than 10 micrometers.

31. A crystalline article, comprising: 40 mol% ≤ SiO2 ≤ 50 mol%; 25 mol% ≤ Al2O3 ≤ 32.5 mol%; and 22.5 mol% ≤ SrO ≤ 30 mol%; wherein Al2O3 ≥ SrO; and wherein the crystalline article comprises at least 90 volume% of crystalline material; and wherein the crystalline material comprises 90 volume% of a single crystal phase.

32. The crystalline article according to claim 31, wherein the crystalline article includes a first major surface and a second major surface opposite the first major surface, and wherein the distance between the first major surface and the second major surface defines the thickness of the crystalline article, the thickness being at most 1 mm.

33. The crystalline article according to claim 32, wherein the crystalline article comprises columnar crystals, wherein most of the columnar crystals are oriented within 15 degrees of the normal to one or both of the first major surface and the second major surface.

34. The crystalline article according to any one of claims 31 to 33, wherein the single crystal phase is Sr(Al2Si2O8).

35. The crystalline article according to any one of claims 31 to 34, wherein the crystalline phase comprises 1 volume% or less of a secondary crystalline phase.

36. The crystalline article according to any one of claims 31 to 35, wherein the secondary crystalline phase is SrSiO3.

37. The crystalline article according to any one of claims 31 to 36, wherein the crystalline article transmits at least 70% of light having a wavelength of 400 nm to 800 nm.

38. The crystalline article according to any one of claims 31 to 37, wherein 0 < Al2O3 – SrO ≤ 5 mol%.

39. The crystalline article according to any one of claims 32 to 38, wherein the crystalline article comprises a first crystalline region extending from the first major surface into the thickness and a second crystalline region extending from the second major surface into the thickness, and wherein the first crystalline region meets the second crystalline region at approximately the midpoint of the thickness.

40. The crystalline article according to any one of claims 31 to 39, comprising other components individually at 1 mol% or less and all other components in total at 5 mol% or less.

41. A crystalline article, comprising: 40 mol% to 50 mol% of SiO2; Al2O3; and SrO; where 0 < Al2O3 – SrO ≤ 5 mol%; wherein the crystalline article comprises a first major surface, a second major surface, and a thickness, the second major surface being opposite the first major surface, and the thickness being the distance between the first major surface and the second major surface; and wherein the thickness is 1 mm or less.

42. The crystalline article according to claim 41, wherein SiO2 + Al2O3 + SrO ≥ 85 mol%.

43. The crystalline article according to claim 41 or claim 42, wherein the crystalline article comprises at least 90 vol% of a crystalline phase.

44. The crystalline article according to claim 43, wherein the crystalline phase comprises at least 90 vol% of a first crystal structure.

45. The crystalline article according to claim 44, wherein the first crystal structure is Sr(Al2Si2O8).

46. The crystalline article according to claim 44 or claim 45, wherein the crystalline phase comprises no more than 1 vol% of a second crystal structure.

47. The crystalline article according to claim 46, wherein the second crystal structure is SrSiO3.

48. The crystalline article according to any one of claims 41 to 47, further comprising a first crystalline region and a second crystalline region, wherein the first crystalline region comprises columnar crystals extending from the first major surface toward the midpoint of the thickness, and wherein the second crystalline region comprises columnar crystals extending from the second major surface toward the midpoint of the thickness.

49. The crystalline article according to claim 48, wherein the columnar crystals are oriented within 15° of the normal to the respective first major surface and second major surface.

50. The crystalline article according to any one of claims 41 to 49, wherein at least 70% of the light having a wavelength in the range of 400 nm to 800 nm incident on one of the first major surface or the second major surface of the crystalline article is transmitted through the crystalline article to the other of the first major surface or the second major surface.

51. A method of manufacturing a crystalline article, comprising: nucleating first columnar crystals on a first major surface of a glass article and second columnar crystals on a second major surface of the glass article until the first columnar crystals meet the second columnar crystals to form the crystalline article; wherein both the first columnar crystals and the second columnar crystals extend inwardly from the respective first major surface and the second major surface; wherein the glass article comprises SiO2, Al2O3 and SrO; wherein 40 mol % ≤ SiO2 ≤ 50 mol %; and Where 0≤Al2O3–SrO≤5 mol%.

52. The method of claim 51, wherein nucleating comprises heat treating the glass article at a temperature in the range of 1010°C to 1080°C.

53. The method of claim 52, wherein the heat treatment is performed for a period of 1 hour to 5 hours.

54. The method of claim 52 or claim 53, further comprising polishing at least one of the first major surface or the second major surface by grinding a portion of at least one of the first major surface or the second major surface after heat treating.

55. The method of any one of claims 51 to 54, wherein the thickness is 1 mm or less.

56. The method of any one of claims 51 to 55, wherein the first columnar crystals and the second columnar crystals comprise at least 90 volume percent of the first crystal structure.

57. The method of claim 56, wherein the first crystal structure is Sr(Al2Si2O8).

58. The method of claim 56 or claim 57, wherein the first columnar crystals and the second columnar crystals contain 1 volume % or less of the second crystal structure.

59. The method of claim 58, wherein the second crystal structure is SrSiO3.

60. The process of any one of claims 51 to 59, wherein 25 mol%≤Al2O3≤32.5 mol%, and 22.5 mol%≤SrO≤30 mol%.