Insulating resin composition, cured product, winding coil, and rotating machine
By using epoxy-based and meth(acryloyl)-based thermosetting resins and biomass materials to prepare insulating resins, the problems of volatilization and viscosity of the insulating resin during the curing process are solved, and the surface contact properties and mechanical strength are improved, making it suitable for Insulated coils for large rotating machines.
Patent Information
- Application Number
- CN202280074902.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-10
- Publication Date
- 2024-10-11
AI Technical Summary
During the curing process of existing insulating resins, part of the monofunctional vinyl monomers volatilize, resulting in sticky residue on the surface. Moreover, the use of traditional organic solvents is limited by environmental loads, making it difficult to meet the requirements for efficient penetration and low viscosity.
Using epoxy and meth (acryloyl) thermosetting resins, free radical polymerization initiators and curing agents for epoxy, combined with biomass materials to prepare multifunctional and monofunctional vinyl monomers , optimize the viscosity and curing reaction of the insulating resin and reduce the formation of volatiles.
It improves the surface contact properties of the cured product of the insulating resin, reduces the formation of lumpy cured products, enhances the mechanical strength and heat resistance, reduces the environmental load, and is suitable for insulating coils of large rotating machines.
Smart Images

Figure CN118765296A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an insulating resin composition, a cured product, a winding coil, and a rotating machine. Background Art
[0002] Patent Document 1 discloses an example of a solvent-free varnish composition used as an insulating varnish. In the solvent-free varnish composition, a monofunctional vinyl monomer such as 2-hydroxyethyl methacrylate (2-HEMA) is added as a reactive diluent for viscosity adjustment. After the solvent-free varnish composition is immersed in a coil, it is heated to be cured.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2017 / 061006 Summary of the invention
[0006] Problems to be solved by the invention
[0007] However, in the insulating resin composition such as the solvent-free varnish composition of patent document 1, a part of the monofunctional vinyl monomer can volatilize in the curing furnace during curing heating. Among them, as for the 2-hydroxyethyl methacrylate used as the monofunctional vinyl monomer, it has the characteristics of its molecular structure, that is, it has a hydroxyl group with a high degree of freedom in a relatively short hydrocarbon main chain, so it has high hydrophilicity. Therefore, 2-hydroxyethyl methacrylate reacts easily with moisture in the air and can be reattached on the surface of the cured product. As a result, stickiness sometimes remains on the surface of the cured product. In addition, in order to be able to cope with the environmental control that tends to be strengthened due to concern for international environmental issues in recent years, the necessity of insulating resins such as reducing raw materials from petroleum is increased.
[0008] The present disclosure relates to solving such problems. The present disclosure provides an insulating resin composition and a cured product thereof that use a biomass material as a raw material and further improves the surface touchability of the cured product, as well as a winding coil with excellent surface touchability and a rotating machine using the same.
[0009] Means for solving problems
[0010] The insulating resin composition disclosed herein comprises: a thermosetting resin having both an epoxy group and a methyl (acryloyl) group, a free radical polymerization initiator and a curing agent for the epoxy group, a multifunctional vinyl monomer using a biomass material as a raw material, and a monofunctional vinyl monomer using a biomass material as a raw material, wherein the monofunctional vinyl monomer comprises both a vinyl monomer having an isobornyl skeleton and a vinyl monomer having a cyclic ether skeleton of a saturated hydrocarbon, and the biomass degree is greater than 60% and less than 84%.
[0011] The cured product according to the present disclosure is obtained by curing the above-mentioned insulating resin composition.
[0012] The wound coil according to the present disclosure is impregnated with the above-mentioned insulating resin composition.
[0013] The rotating machine according to the present disclosure is a rotating machine used in a hoisting machine for driving a car of a rope-type elevator, and includes a stator using the above-mentioned winding coil.
[0014] Effects of the Invention
[0015] According to the insulating resin composition of the present disclosure, the surface touchability of the cured product is further improved while using the biomass material as the raw material. In addition, the surface touchability of the winding coil using the biomass material as the raw material is further improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a conceptual diagram showing an example of a state in which an insulating resin is cured.
[0017] Figure 2 It is a cross-sectional view of the hoisting machine involved in Embodiment 1. DETAILED DESCRIPTION
[0018] Implementation method 1.
[0019] The following is a description of the method for implementing the object of the present disclosure. It should be noted that the object of the present disclosure is not limited to the following embodiments, and any constituent element of the embodiments may be modified or omitted without departing from the gist of the present disclosure. In addition, the embodiments and examples in the present disclosure are illustrative in all aspects and should not be interpreted restrictively.
[0020] In Embodiment 1, a liquid insulating resin composition (X) and a cured product thereof (Y) are described. In addition, a winding coil for a rotating machine using the insulating resin composition (X) and a rotating machine using the same for a stator are also described.
[0021] 1. Insulating resin composition (X) and cured product (Y)
[0022] The insulating resin composition (X) of embodiment 1 is used, for example, in the coil of a rotating machine to maintain insulation and mechanical strength. The coil is formed by winding a winding such as an enameled wire around an iron core. The device to which the coil is applied is not limited to a specific device. The coil is applied to, for example, an electric motor such as a motor, or a rotating machine such as a generator. The coil is applied to, for example, a hoist of an elevator or an electric compressor. As for the insulating resin composition (X), the coil is immersed in the coil by, for example, an immersion method in which the coil is immersed in an immersion tank filled with the insulating resin composition (X). As for the insulating resin composition (X), it is cured by heating in a curing furnace to become a cured product (Y).
[0023] Here, the insulating resin impregnated to ensure the insulation and mechanical strength of the coil of the rotating machine is generally high in viscosity, and in this case, it is difficult to make the insulating resin penetrate between the windings and into the inside of the coil. In particular, in a large rotating machine, the coil is long and thick, so it is more difficult for the high-viscosity insulating resin to penetrate.
[0024] In particular, when insulating resin is applied to a large rotating machine, a material design suitable for the coil of the large rotating machine is required. As a method of filling the insulating resin between the windings in the coil of the rotating machine, there are dipping methods or titration methods. For example, in coils with a relatively small size and low winding density used in compressors, both the dipping method and the titration method can be used. On the other hand, in large rotating machines used in generators or hoists, if the titration method is used, it is difficult to evenly adhere the insulating resin between the windings and even to the inside of the coil. Therefore, in large rotating machines, the dipping method under atmosphere or vacuum is generally used.
[0025] The impregnation method is a method of impregnating the coil in a tank or impregnation tank filled with insulating resin under the atmosphere or in a vacuum so that the insulating resin is impregnated between the wound wires. Among them, when the coil impregnated by the impregnation method is lifted from the impregnation tank, a large amount of excess insulating resin is attached to the winding wire, the iron core and other components of the coil. In many cases, the coil lifted from the impregnation tank is put into a curing furnace for curing heating while the excess insulating resin is attached. Therefore, the excess insulating resin attached to the coil is directly cured, for example, a block-shaped solidified product can be formed at the bottom of the coil, the depression of the iron core, or on other components. In addition, the insulating resin whose viscosity is reduced due to the curing heating and drips down below the coil sometimes forms a large resin retention in the curing furnace.
[0026] As for the block-like solidified materials formed at the bottom of the coil, in the depression of the core, or on other components, the thermal stress caused by curing shrinkage and the like may damage the winding and components, which may become the main factor for reducing the insulation. Furthermore, the block-like solidified materials become an obstacle to the operation of assembling the coil to the fixed component, so it becomes necessary to remove the block-like solidified materials. In addition, the resin retention formed in the curing furnace sometimes produces smoke due to the heat of curing. The resin retention becomes a huge solidified material formed on the hearth of the curing furnace, so regular cleaning of the curing furnace becomes indispensable. Such problems are particularly prominent in large rotating machines, and the necessity of low-viscosity insulating resin that can suppress the formation of block-like solidified materials and resin retention increases.
[0027] In order to reduce the viscosity of such insulating resins and improve permeability, etc., it is effective to add organic solvents such as styrene or vinyltoluene to the insulating resin. However, with the increasing concern about environmental issues in recent years, the demand for reducing the environmental load in insulating resins has increased, so it is preferred to suppress the use of these organic solvents. Therefore, instead of adding these organic solvents, a low-molecular material having an active group that can contribute to the curing reaction and can reduce the volatile substances caused by the curing heating, that is, a reactive diluent, can be added to the insulating resin to adjust the viscosity. As such a reactive diluent, a monofunctional monomer, especially 2-hydroxyethyl methacrylate, is effective.
[0028] Figure 1 This is a conceptual diagram showing an example of the state of insulating resin curing. Figure 1 , an example of an insulating resin 2 being cured on the surface of the winding of the coil 1 is shown. During the curing reaction, although most of the reactive diluent added to the insulating resin 2 is absorbed into the cured product, a part 3 of the reactive diluent volatilizes and fills the interior of the curing furnace. Here, the air in the furnace contains moisture 4. It should be noted that a thin film 5 made of paraffin may also be formed on the surface of the cured insulating resin 2.
[0029] As for 2-hydroxyethyl methacrylate, it has a high hydrophilicity due to the characteristics of its molecular structure, that is, a hydroxyl group with a high degree of freedom in a relatively short hydrocarbon main chain. Therefore, when 2-hydroxyethyl methacrylate is used as a reactive diluent, a part of the volatilized material easily reacts with moisture in the air and can be reattached on the surface of the cured product. As a result, sometimes stickiness remains on the surface of the cured product. The stickiness on the surface of the cured product becomes an obstacle to the subsequent process of the impregnation treatment, that is, the assembly operation, so for the insulating resin, it is required to eliminate the stickiness on the surface of the cured product and improve the touchability.
[0030] The insulating resin composition (X) of embodiment 1 includes: a thermosetting resin (A) having both an epoxy group and a methacryloyl group, a free radical polymerization initiator and a curing agent for the epoxy group (B), a multifunctional vinyl monomer (C) using a biomass material as a raw material, and a monofunctional vinyl monomer (D) using a biomass material as a raw material. The monofunctional vinyl monomer (D) has a cyclic structure in the molecule. The monofunctional vinyl monomer (D) includes a vinyl monomer (D-1) having an isobornyl skeleton and a vinyl monomer (D-2) having a cyclic ether skeleton of a saturated hydrocarbon. Here, the so-called methacryloyl group represents an acryloyl group or a methacryloyl group. In addition, in the present disclosure, the numerical range represented by "x to y" represents a numerical range including a lower limit x and an upper limit y.
[0031] In order to suppress the excessive adhesion of the insulating resin composition (X) to the coil pulled out from the dipping tank after dipping by the dipping method, it is preferred that the viscosity is low and the liquid removal property is good. The overall viscosity of the insulating resin composition (X) is preferably 10 mPa·s to 200 mPa·s, more preferably 10 mPa·s to 100 mPa·s, and even more preferably 15 mPa·s to 50 mPa·s.
[0032] 1.1. Thermosetting resin (A)
[0033] The thermosetting resin (A) includes a resin having both an epoxy group and a meth(acryloyl) group in one molecule. The thermosetting resin (A) may be used alone or mixed with a second resin containing one or both of an epoxy group and a meth(acryloyl) group in one molecule. The second resin may be a mixture of a plurality of resins.
[0034] The thermosetting resin (A) promotes the three-dimensional crosslinking reaction caused by the addition reaction of free radicals generated by the organic peroxide using the meth(acryloyl) group as the reactive group and the ring-opening polymerization reaction using the epoxy group as the reactive group, thereby promoting the curing reaction and improving the heat resistance and mechanical strength of the cured product.
[0035] The thermosetting resin (A) has a number average molecular weight (Mn) of 15,000 or less, preferably 1,000 to 10,000, and more preferably a viscosity of 10,000 mPa·s or less at 60° C., from the perspective of ease of viscosity adjustment.
[0036] The epoxy equivalent of the thermosetting resin (A) contained in the insulating resin composition (X) is preferably 500 to 5000, more preferably 1000 to 4000. By controlling the epoxy equivalent within the above range, the curing speed can be increased without reducing the usable time of the insulating resin composition (X), and the crosslinking density of the cured product (Y) can be increased.
[0037] 1.2. Free radical polymerization initiator and epoxy curing agent (B)
[0038] In order to cure the thermosetting resin (A) and the monofunctional vinyl monomer (D), an organic peroxide as a radical polymerization initiator that acts mainly on meth(acryloyl) groups and a curing catalyst for epoxy groups are used in combination.
[0039] 1.2.1. Organic peroxides
[0040] Organic peroxide is mainly used as a reaction initiator of methyl (acryloyl) group, and substances known in the technical field can be used. As far as organic peroxide is concerned, as long as the 10-hour half-life temperature is above 40°C, there is no particular limitation. From the perspective of shortening the curing time and adjusting the curing temperature, the preferred 10-hour half-life temperature is 100°C to 170°C. As examples of these organic peroxides, peroxides of ketone peroxide system, peroxyketal system, hydroperoxide system, dialkyl peroxide system, diacyl peroxide system, peroxyester system, peroxydicarbonate system, etc. can be used. These organic peroxides can be used alone, or two or more kinds can be mixed and used.
[0041] Examples of organic peroxides having such a 10-hour half-life temperature include 1,1-di(tert-butylperoxy)cyclohexane, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-butylperoxy)-2-methylcyclohexane, 2,2-di(4,4-di-(butylperoxy)cyclohexyl)propane, 4,4-di-(tert-butylperoxy)butyl valerate, 2,2-di-(tert-butylperoxy)butane, tert-hexyl peroxyisopropyl monocarbonate, tert-butylperoxymaleic acid, tert-butylperoxy-3,5,5-trimethylhexanoic acid, tert-butylperoxylauric acid, tert-butylperoxyisopropyl monocarbonate, benzene peroxide, and the like. tert-Butyl formate, tert-butyl peroxyacetate, tert-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, tert-butyl peroxy-2-ethylhexyl monocarbonate, di(2-tert-butylperoxyisopropyl)benzene, dicumyl peroxide, di-tert-hexyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, p-menthane hydroperoxide, tert-butyl peroxyallyl monocarbonate, methyl ethyl ketone peroxide, 1,1,3,3-tetramethylbutyl hydroperoxide, tert-butyl hydroperoxide, isopropylbenzene hydroperoxide, diisopropylbenzene hydroperoxide, etc. These may be used alone or in combination of two or more.
[0042] The amount of the organic peroxide in the insulating resin composition (X) is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the total of the thermosetting resin (A), the multifunctional vinyl monomer (C) and the monofunctional vinyl monomer (D). If the amount of the organic peroxide is less than 0.1 parts by mass, the crosslinking density becomes small and the required mechanical strength cannot be obtained. On the other hand, if the amount of the organic peroxide is more than 10 parts by mass, the usable time of the insulating resin composition tends to be significantly shortened.
[0043] 1.2.2. Curing agents for epoxy groups
[0044] The curing agent for epoxy groups can use substances known in the art. As the curing agent for epoxy groups, for example, amine compounds, borate compounds, organometallic compounds, organophosphorus compounds, quaternary ammonium salts, quaternary phosphonium salts, amine complexes, imidazole compounds, compounds containing transition metals such as titanium and cobalt, acid anhydrides, imidazole compounds, polythiol compounds, phenols, Lewis acids, isocyanate compounds, etc. can be listed. These can be used alone, or two or more can be mixed and used.
[0045] Specific examples of the amine curing agent include tertiary amines and tertiary amine salts. For example, lauryl dimethylamine, N,N-dimethylcyclohexylamine, N,N-dimethylbenzylamine, N,N-dimethylaniline, (N,N-dimethylaminomethyl)phenol, 2,4,6-tris(N,N-dimethylaminomethyl)phenol, 1,8-diazabicyclo[5.4.0]undecene-7 (DBU), 1,5-diazabicyclo[4.3.0]nonene-5 (DBN), ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, dipropylenediamine, polyetherdiamine, 2,5-dimethylhexamethylenediamine, trimethylhexamethylenediamine, diethylenetriamine, iminobispropylamine, Bis(hexamethyl)triamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, aminoethylethanolamine, tri(methylamino)hexane, dimethylaminopropylamine, diethylaminopropylamine, methyliminobispropylamine, menthanediamine, isophoronediamine, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, N-aminoethylpiperazine, 3,9-bis(3-aminopropyl)-2,4,8,10-tetraoxaspiro[5,5]undecane, m-xylene diamine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldiphenylmethane, dicyandiamide, organic acid dihydrazide, etc. Examples of tertiary amine salts include carboxylates, sulfonates, and inorganic acid salts of the above-mentioned tertiary amines. Examples of carboxylates include salts of carboxylic acids having 1 to 30 carbon atoms (especially 1 to 10 carbon atoms) such as octanoates (especially salts of fatty acids). Examples of sulfonates include p-toluenesulfonates, benzenesulfonates, methanesulfonates, ethanesulfonates, etc. Representative specific examples of tertiary amine salts include salts of 1,8-diazabicyclo[5.4.0]undecene-7 (DBU) (e.g., p-toluenesulfonate, octanoate), etc. However, these are merely examples. Although amine curing agents other than these are used, they do not deviate from the scope of the present disclosure.
[0046] Examples of boric acid esters include trimethyl borate, triethyl borate, tripropyl borate, tributyl borate, and cyclic boric acid ester compounds. However, these are merely examples. Although boric acid esters other than these may be used, this does not deviate from the scope of the present disclosure.
[0047] Examples of organometallic compounds include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, zinc stearate, and aluminum acetylacetonate complexes. However, these are merely illustrative. Although organometallic compounds other than these may be used, they do not depart from the scope of the present disclosure.
[0048] Examples of the organophosphorus compound include tetraphenylphosphonium tetraphenylborate and triphenylphosphine. However, these are merely examples. Although organophosphorus compounds other than these may be used, this does not deviate from the scope of the present disclosure.
[0049] As the example of quaternary ammonium salt, tetramethylammonium chloride, tetramethylammonium bromide, tetramethylammonium iodide, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium iodide, tetrabutylammonium chloride, tetrabutylammonium bromide, tetrabutylammonium iodide, triethylbenzylammonium chloride, triethylbenzylammonium bromide, triethylbenzylammonium iodide, triethylphenethylammonium chloride, triethylphenethylammonium bromide etc. can be listed. However, these are only illustrative after all. Although the quaternary ammonium salts other than these are used, it does not depart from the scope of the present disclosure.
[0050] As examples of quaternary phosphonium salts, tetrabutyl phosphonium chloride, tetrabutyl phosphonium iodide, tetrabutyl phosphonium acetate, tetraphenyl phosphonium chloride, tetraphenyl phosphonium bromide, tetraphenyl phosphonium iodide, ethyl triphenyl phosphonium chloride, ethyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium iodide, ethyl triphenyl phosphonium acetate, ethyl triphenyl phosphonium phosphate, propyl triphenyl phosphonium chloride, propyl triphenyl phosphonium bromide, propyl triphenyl phosphonium iodide, butyl triphenyl phosphonium chloride, butyl triphenyl phosphonium bromide, butyl triphenyl phosphonium iodide, etc. can be listed. However, these are only examples after all. Although quaternary phosphonium salts other than these are used, it does not depart from the scope of the present disclosure.
[0051] Examples of amine complexes include complexes of boron halides such as boron trifluoride, boron trichloride and boron tribromide with amine compounds, i.e., boron halide amine complexes. Examples of amine compounds include aliphatic tertiary amines such as trimethylamine, tri-n-propylamine, N,N-dimethyloctylamine, and N,N-dimethylbenzylamine, aromatic tertiary amines such as N,N-dimethylaniline, heterocyclic tertiary amines such as substituted or unsubstituted imidazole or pyridine alkylated at the 1-position, aliphatic primary amines such as monoethylamine and n-hexylamine, aliphatic primary amines containing aromatic rings such as benzylamine, aromatic primary amines such as aniline, and secondary amines such as piperidine. As representative specific examples of the halogenated boron amine complex, boron trifluoride monoethylamine complex, boron trifluoride diethylamine complex, boron trifluoride isopropylamine complex, boron trifluoride chloroaniline complex, boron trifluoride-triallylamine complex, boron trifluoride benzylamine complex, boron trifluoride aniline complex, boron trichloride monoethylamine complex, boron trichloride phenol complex, boron trichloride piperidine complex, boron trichloride dimethyl sulfide complex, boron trichloride N, N-dimethyloctylamine complex, boron trichloride N, N-dimethyldodecylamine complex, boron trichloride N, N-diethyldioctylamine complex, etc. can be listed. However, these are only examples after all. Although amine complexes other than these are used, it does not deviate from the scope of the present disclosure.
[0052] Examples of imidazole compounds include 2-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, 2,4-diamino-6-(2'-methylimidazole (1'))ethyl-s-triazine. 2,4-diamino-6 (2'-undecyl imidazole (1')) ethyl-s-triazine, 2,4-diamino-6 (2'-ethyl, 4-methyl imidazole (1')) ethyl-s-triazine, 2,4-diamino-6 (2'-methyl imidazole (1')) ethyl-s-triazine.isocyanuric acid adduct, 2-methyl imidazole isocyanuric acid 2:3 adduct, 2-phenyl imidazole isocyanuric acid adduct, 2-phenyl-3,5-dihydroxymethyl imidazole, 2-phenyl-4-hydroxymethyl-5-methyl imidazole, 1-cyanoethyl-2-phenyl-3,5-dicyanoethoxymethyl imidazole, etc. However, these are only examples. Although imidazole curing agents other than these are used, it does not deviate from the scope of the present disclosure.
[0053] Specific examples of anhydride curing agents include methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, etc. However, these are merely examples. Although anhydride curing agents other than these may be used, it does not deviate from the scope of the present disclosure.
[0054] The amount of the epoxy curing agent can be appropriately adjusted according to the type of the thermosetting resin (A) and the type of the curing agent. The amount of the curing agent is preferably about 0.5 equivalents or more and 2 equivalents or less relative to the epoxy equivalent of the thermosetting resin (A). If the amount of the curing agent is less than 0.5 equivalents, the curing of the thermosetting resin (A) may not be fully carried out. If the amount of the curing agent exceeds 2 equivalents, the heat resistance and mechanical properties of the cured product may be reduced.
[0055] 1.2.3. Curing accelerators for epoxy groups
[0056] In addition to the curing agent for epoxy groups mentioned above, a curing accelerator may be used in combination to promote the curing reaction or to control the reaction. As a curing accelerator, for example, tertiary amines and their salts, quaternary ammonium compounds, imidazoles, alkali metal alkoxides, etc. may be cited. However, these are merely illustrative. Although curing accelerators other than these are used, they do not deviate from the scope of the present disclosure.
[0057] The amount of the curing accelerator is preferably 0.01% by mass to 30% by mass (more preferably 0.05% by mass to 20% by mass) relative to the mass of the thermosetting resin (A). If the amount is less than 0.01% by mass, the accelerator effect may be small. If the amount exceeds 30% by mass, the storage stability of the insulating resin composition (X) and the moldability of the cured product may be reduced.
[0058] 1.3. Multifunctional vinyl monomer (C)
[0059] The multifunctional vinyl monomer (C) uses biomass materials as part of its raw materials. The multifunctional vinyl monomer (C) is arbitrarily formulated as one of the reactive diluents of the insulating resin composition (X). As far as the multifunctional vinyl monomer (C) is concerned, there is no particular limitation as long as it contributes to the free radical polymerization reaction, and it is preferably a substance containing two methyl (acryloyl) groups or allyl groups as reactive groups in one molecule. For such a multifunctional vinyl monomer (C), since there are two reactive groups that contribute to the reaction in one molecule, it is polymerized and completely absorbed during the curing treatment of the insulating resin composition (X), and the volatilization during the curing treatment is also significantly less. Therefore, by adding it as a reactive diluent, the insulating resin composition (X) can be made low in viscosity, and the re-adsorption caused by the volatilization during the curing heating is also suppressed. In addition, as far as the multifunctional vinyl monomer (C) is concerned, by having multiple reactive groups, it actively participates in the polymerization reaction of the insulating resin composition (X), and can promote the three-dimensional crosslinking of the insulating resin composition (X). Therefore, the heat resistance and mechanical strength of the cured product (Y) can also be improved.
[0060] The amount of the polyfunctional vinyl monomer (C) added may be within the range that can ensure the amount of the monofunctional vinyl monomer (D). From the viewpoint of mechanical strength and heat resistance, it is preferably within the range of 3wt% to 20wt% of the total of the thermosetting resin (A), the polyfunctional vinyl monomer (C) and the monofunctional vinyl monomer (D).
[0061] 1.4. Monofunctional vinyl monomer (D)
[0062] The monofunctional vinyl monomer (D) uses biomass materials as part of its raw materials. The monofunctional vinyl monomer (D) is used mainly for adjusting the viscosity of the insulating resin composition (X) in addition to adjusting the crosslinking structure. In order to maintain the usable time of the insulating resin composition (X), the monofunctional vinyl monomer (D) is preferably a monofunctional vinyl monomer having one functional group that contributes to the reaction in one molecule.
[0063] As the monofunctional vinyl monomer (D), a low-viscosity vinyl monomer having an ether bond or an ester bond and a cyclic structure is used. Among them, a vinyl monomer (D-1) having an isobornyl skeleton and a vinyl monomer (D-2) having a cyclic ether skeleton of a saturated hydrocarbon are used in combination. Examples of the vinyl monomer (D-1) having an isobornyl skeleton include isobornyl methacrylate and isobornyl acrylate. Examples of the vinyl monomer (D-2) having a cyclic ether skeleton of a saturated hydrocarbon include tetrahydrofurfuryl methacrylate and tetrahydrofurfuryl acrylate.
[0064] As for the amount of the monofunctional vinyl monomer (D), it is preferred to use as much as possible from the viewpoint of increasing the biomass degree of the insulating resin composition (X) and improving the environmental load reduction effect, and from the viewpoint of improving the deliquescence of the insulating resin composition (X) when the coil is lifted from the dipping tank and inhibiting the formation of blocky solidified products on the coil and other constituent members. On the other hand, as for the monofunctional vinyl monomer (D), although it contributes to the increase of crosslinking points, it is low molecular weight and part of it volatilizes during curing heating, so the entire amount does not contribute to the curing reaction. Therefore, if the amount is too much, the mechanical strength of the cured product (Y) is reduced. That is, as for the amount of the monofunctional vinyl monomer (D), it is necessary to adjust it to a range that can achieve the opposite required functions, that is, the improvement of the biomass degree and the inhibition of the formation of blocky solidified products and the mechanical strength of the cured product (Y). From the viewpoint of improving the biomass degree and inhibiting the formation of blocky solidified products, the amount of the monofunctional vinyl monomer (D) is preferably more than 60wt% of the total amount of the insulating resin composition (X), preferably more than 65wt%. On the other hand, from the viewpoint of the mechanical strength of the cured product (Y), the amount of the monofunctional vinyl monomer (D) is preferably 85 wt% or less, preferably 75 wt% or less, and more preferably 70 wt% or less of the total amount of the insulating resin composition (X). Therefore, in order to achieve both the required two functions, the amount of the monofunctional vinyl monomer (D) is preferably 60 to 85 wt%, preferably 60 to 85 wt%, and more preferably 65 to 85 wt% of the total amount of the insulating resin composition (X).
[0065] Among the monofunctional vinyl monomers (D), monofunctional vinyl monomers having one meth(acryloyl) group or allyl group in one molecule may be combined with the above-mentioned vinyl monomers (D-1) and (D-2). Examples of these monofunctional vinyl monomers include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, lauryl methacrylate, ethoxydiglycol methacrylate, 4-hydroxybutyl methacrylate, n-octyl acrylate, etc. These monofunctional vinyl monomers may be used alone or in combination.
[0066] 2. Method for producing insulating resin composition (X) and cured product (Y) thereof
[0067] 2.1. Insulating resin composition (X)
[0068] The insulating resin composition (X) can be produced by the following production method. The amounts of (A) to (D) are the amounts described in the Examples and Comparative Examples. The mixing method can effectively utilize a method known in the technical field, and is not particularly limited as long as uniform mixing is possible.
[0069] (a) Mixture of thermosetting resin, multifunctional vinyl monomer and monofunctional vinyl monomer
[0070] The thermosetting resin (A) and the multifunctional vinyl monomer (C) are heated to about 50°C to a viscosity that allows fluidity from a semisolid state, and then weighed. The monofunctional vinyl monomer (D) is added thereto, and stirred with a rotational stirrer until a uniform solution is obtained.
[0071] (b) Preparation of insulating resin composition (X)
[0072] In the mixed solution of (A), (C) and (D) prepared in the above (a), a radical polymerization initiator and a curing agent (B) for epoxy groups are uniformly mixed.
[0073] 2.2. Cured product (Y)
[0074] The cured product (Y) is a cured product of the insulating resin composition (X). The cured product (Y) is typically produced by heating the insulating resin composition (X). The cured product (Y) is used in various forms and shapes depending on the application. The cured product (Y) can be formed into a desired shape by various molding methods such as dipping, coating, casting, sheet molding, etc.
[0075] The solidified product (Y) has excellent insulating properties and heat resistance. Therefore, the solidified product (Y) is suitable for applications requiring at least one of insulating properties and heat resistance. The solidified product (Y) is suitable, for example, for insulating components of heavy electrical equipment such as rotating machines and power transmission and transformation equipment. As insulating components, for example, varnish, insulating paint, cable coating materials, insulating sheets, sealing materials, etc. can be cited.
[0076] When the cured product (Y) is a product obtained by impregnating the insulating resin composition (X) in a coil of a rotating machine or the like and then curing it, the impregnation step of the coil is not particularly limited. Here, an example of a production method consisting of five steps including a preheating step and an air cooling step before impregnation, and then an impregnation step, a dripping removal step, and a heating and curing step is described.
[0077] The preheating step is a step of performing an annealing treatment for the purpose of improving the cleaning resistance of the winding wire of the enameled wire or the like. In the preheating step, the coil is heated at a predetermined temperature. The heating temperature in the preheating step is not particularly limited as long as it is a temperature that can improve the cleaning resistance, and for example, the treatment is performed at 150°C.
[0078] The air cooling step is a step of cooling the coil to a predetermined temperature in order to suppress the temperature rise of the insulating resin composition (X). The temperature of the coil after cooling is not particularly limited as long as it is within a temperature range that does not affect the usable life of the insulating resin composition (X), and for example, 30°C to 50°C is suitable.
[0079] In the impregnation process, a treatment method known in the art such as impregnation, titration, pressure impregnation, vacuum impregnation, etc. can be used. Generally, in the case of a coil of a large rotating machine, an impregnation treatment using impregnation or pressure and vacuum impregnation is performed. In the case of an impregnation treatment using impregnation, the coil is quietly immersed in an impregnation tank filled with an insulating resin composition (X). There is no particular limitation on the impregnation time. In particular, for coils that are wound in a row and are tightly wound, the air attached between the enameled wires and the constituent members becomes bubbles and floats to the surface, so it is preferred to immerse until the generation of these bubbles disappears. The time until the generation of bubbles subsides varies depending on the size of the coil. For a large rotating machine, it is about 10 minutes to 60 minutes. From the perspective of efficiency (shortening the time) of the manufacturing process, it is preferably about 15 to 30 minutes. This is because, if the immersion time is less than 10 minutes, the insulating resin composition (X) does not penetrate the entire coil, and even if the bubbles are generated and converged (constricted) for more than 60 minutes of immersion, the amount of the insulating resin composition (X) that penetrates the coil does not increase. As for the immersion temperature, that is, the temperature of the insulating resin composition (X) in the immersion tank, there is no particular limitation as long as it is a temperature range where thickening caused by curing does not begin. In a large amount of insulating resins, it is set to room temperature 25°C to 60°C. Since the insulating resin composition (X) has a low viscosity, it can also be immersed at room temperature 25°C.
[0080] In the heat curing step, the insulating resin composition (X) impregnated in the coil by the impregnation step is heated in a curing furnace and cured to form a cured product (Y). The heating temperature in the heat curing step is not particularly limited as long as it is above the reaction start temperature (half-life temperature) of the reaction initiator added to the insulating resin composition (X), and is generally 130°C to 180°C, preferably 140°C to 170°C. Generally, the heating time in the heat curing step is affected by the curing speed of the insulating resin composition (X) and the amount of adhesion to the coil, and also varies depending on the composition of the raw materials. In addition, the time required for curing depends on the heating temperature, and generally the time until complete curing is short at a high temperature. Therefore, the heating temperature and heating time in the heat curing step are set to the temperature and time required for complete curing according to the composition of the insulating resin composition (X). However, when the heating temperature or heating time is insufficient, the insulating resin composition (X) cannot be completely cured, and uncured parts may be generated. In this case, various properties such as electrical properties, mechanical properties, and heat resistance may be reduced in the cured product (Y). On the other hand, when the heating temperature or heating time is excessive, the cross-linking reaction caused by the curing heating is unbalanced, which sometimes becomes the cause of cracks in the cured product (Y). The heating temperature and heating time are set within the range where these problems do not occur. The insulating resin composition (X) disclosed in the present invention is completely cured in 30 minutes to 8 hours at 130 to 180°C. If the curing time is less than 30 minutes, complete curing cannot be achieved. On the other hand, with respect to the mechanical strength (fixing strength of the wire) of the cured product (Y), it slowly appears and improves after curing, and tends to converge after a specified time, here after 4 hours. Therefore, from the viewpoint of complete curing and strength convergence, the heating time in the heat curing process is preferably 1 to 4 hours, and more preferably 1 to 2 hours.
[0081] 2.3. Winding coil for rotating machine and stator using the same
[0082] The insulating resin composition (X) of the first embodiment is suitable for use in, for example, a large rotating machine for a hoisting machine of a rope elevator.
[0083] Figure 2 It is a cross-sectional view of the hoisting machine 10 according to the first embodiment.
[0084] Figure 2 The hoisting machine 10 shown in FIG. 1 includes a rotating portion 11 , a braking portion 12 , and a motor portion 13 .
[0085] The rotating part 11 includes a sheave 14, a rotor 15, a brake disc 16, and a rotating shaft 17. The sheave 14, the rotor 15, and the brake disc 16 are coaxially connected via the rotating shaft 17. A main rope (not shown) is wound around the sheave 14. The elevator car (not shown) supported by the main rope is driven by friction between the main rope and the sheave 14.
[0086] The brake unit 12 includes a movable brake shoe (not shown). The brake unit 12 generates a force for driving the rotating unit 11 by friction generated by pressing the brake shoe against the brake disc 16 .
[0087] The motor unit 13 includes a frame 18 and a stator 19. The stator 19 is fixed to the frame 18 by press-fitting or shrink-fitting. The stator 19 includes a ring-shaped iron core 20. A winding 21 is wound around each tooth of the iron core 20. The winding 21 and the iron core 20 are insulated by an insulator 22. The winding 21 is fixed by the insulator 22. The windings 21 wound around each tooth are connected to each other in a set order, and magnetic flux is generated by energizing.
[0088] The stator 19 is manufactured by, for example, a method including the following steps. First, a bare wire insulated and coated with enamel is prepared. The bare wire is conductive. The material of the bare wire is, for example, copper, aluminum, silver, etc. There is no particular limitation on the type of enamel, and polyesterimide, polyamideimide, polyamide, etc. are used in combination. Inorganic fillers for improving the insulation withstand voltage may also be included in these layers of insulation coating using enamel. These enameled wires can use enameled wires for motor coils that are generally available on the market. Such an insulated and coated enameled wire is wound around the teeth of each of the cores 20 to form a winding 21. Then, the insulating resin composition (X) is impregnated into the winding 21 by the above-mentioned impregnation process, and the insulating resin composition (X) is cured by a heating and curing process.
[0089] In order to improve the impregnation property of the coil, a low molecular weight monofunctional vinyl monomer (D) is used as a reactive diluent to reduce the viscosity in the insulating resin composition (X). Therefore, even the coil of a large rotating machine with a long coil length and a thick coil can be easily impregnated with the insulating resin composition (X). In addition, since the viscosity of the insulating resin composition (X) is low, the formation of unnecessary block-shaped solidified products is suppressed. As a result, the manufacturability of the large rotating machine is improved.
[0090] 3. Example
[0091] The following examples are given for explanation. However, the following examples do not limit the scope of the present disclosure.
[0092] 3.1. Production of insulating resin composition (X) and cured product (Y) thereof
[0093] The insulating resin composition (X) and the cured product (Y) thereof of each example and each comparative example were produced as follows.
[0094] 3.1.1. Material preparation
[0095] Prepare the following materials.
[0096] Thermosetting resin (A)
[0097] A thermosetting resin having both an epoxy group and a meth(acryloyl) group in one molecule, a number average molecular weight of about 2000, and a viscosity of about 3900 mPa·s at 60°C.
[0098] Curing agent and free radical polymerization initiator for epoxy group (B)
[0099] Curing agent: zinc octoate
[0100] Reaction initiator: 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane
[0101] ·Multifunctional vinyl monomer (C)
[0102] Bisphenol A epoxy acrylate with a weight average molecular weight of about 500
[0103] ·Monofunctional vinyl monomer (D)
[0104] (D-1) Isobornyl methacrylate from biomass
[0105] (D-2) Tetrahydrofurfuryl methacrylate from biomass
[0106] (D-3) 2-Hydroxyethyl Methacrylate (2-HEMA)
[0107] 3.1.1.1. Examples 1 to 9
[0108] The thermosetting resin (A) and the multifunctional vinyl monomer (C) are preheated to 40°C in a manner to form a viscosity that is easy to stir, and the thermosetting resin (A), the multifunctional vinyl monomer (C) and the monofunctional vinyl monomer (D) are weighed according to the proportions shown in Table 1 below. Next, the weighed thermosetting resin (A), the multifunctional vinyl monomer (C) and the monofunctional vinyl monomer (D) are all mixed and stirred using a self-rotating revolution stirrer to obtain a uniform mixed solution. To the mixed solution, a curing agent for epoxy groups and a free radical polymerization initiator (B) are added in a manner to form a ratio shown in Table 1 below to obtain an insulating resin composition (X).
[0109] [Table 1]
[0110]
[0111] It should be noted that in Table 1, the weight percentage (wt%) of the reaction initiator represents the ratio relative to the total weight of the thermosetting resin (A) and the monofunctional vinyl monomer (D). In addition, in Table 1, 1phr represents the amount of 1 part by mass of the curing agent to be mixed with 100 parts by mass of the total of the thermosetting resin (A), the multifunctional vinyl monomer (C) and the monofunctional vinyl monomer (D). In addition, in the column of "Main Component" of the monofunctional vinyl monomer (D) in Table 1, "(D-1), (D-2)" indicates that the monofunctional vinyl monomer (D) contains both isobornyl methacrylate (D-1) and tetrahydrofurfuryl methacrylate (D-2). In this column, "(D-3)" indicates that the monofunctional vinyl monomer (D) uses 2-HEMA (D-3) instead of isobornyl methacrylate (D-1) and tetrahydrofurfuryl methacrylate (D-2). In this column, "(D-1)" means that the monofunctional vinyl monomer (D) contains isobornyl methacrylate (D-1) and does not contain tetrahydrofurfuryl methacrylate (D-2). In this column, "(D-2)" means that the monofunctional vinyl monomer (D) contains tetrahydrofurfuryl methacrylate (D-2) and does not contain isobornyl methacrylate (D-1).
[0112] 3.1.1.2. Comparative Examples 1 to 4
[0113] Insulating resin compositions were prepared in the same manner as in Examples 1 to 9 according to the blending amounts shown in Table 1. As shown in Table 1, in Comparative Examples 1 and 2, the total blending amount of (D-1) and (D-2) exceeded 85 wt % of the total amount of the insulating resin composition (X). In Comparative Examples 3 and 4, the total blending amount of (D-1) and (D-2) was less than 60 wt % of the total amount of the insulating resin composition (X).
[0114] 3.1.1.3. Comparative Examples 5 and 6
[0115] An insulating resin composition (X) was prepared in the same manner as in Example 3 except that 2-HEMA (D-3) was used as the monofunctional vinyl monomer (D) instead of isobornyl methacrylate (D-1) and tetrahydrofurfuryl methacrylate (D-2) in the amounts shown in Table 1.
[0116] 3.1.1.4. Comparative Example 7
[0117] An insulating resin composition (X) was prepared in the same manner as in Example 3 except that only isobornyl methacrylate (D-1) was used as the monofunctional vinyl monomer (D) in the amounts shown in Table 1.
[0118] 3.1.1.5. Comparative Example 8
[0119] An insulating resin composition (X) was prepared in the same manner as in Example 3 except that only tetrahydrofurfuryl methacrylate (D-2) was used as the monofunctional vinyl monomer (D) in the amounts shown in Table 1.
[0120] 3.2. Evaluation
[0121] The insulating resin composition (X) and its cured product (Y) were evaluated as follows.
[0122] 3.2.1. Biomass
[0123] The biomass content of the insulating resin composition (X) is 14 The number of C is calculated. The measurement method is based on the method of ASTM D6866. The prepared insulating resin composition (X) is subjected to oxidation treatment to carbon dioxide or graphitize, and then dissolved in scintillation liquid to prepare a sample for Liquid Scintil lat ion Counter (LSC) measurement. Then, the radioactive carbon in this sample is measured using a liquid scintillation counter. 14 The number of C is determined by the total carbon number ( 12 C. 13 C. 14 The biomass degree of the insulating resin composition (X) was determined by the ratio of 14C in the composition. The results are shown in the "Biomass Degree" column of Table 1. 14 The measurement method of C is not limited to the above method, and for example, accelerator mass spectrometry (AMS) may be used.
[0124] 3.2.2. Viscosity
[0125] The viscosity of the insulating resin composition (X) was measured using an E-type viscometer. The results of the measurement at room temperature are shown in the column of "overall viscosity" in Table 1.
[0126] 3.2.3. Mechanical strength (helical coil fixing force)
[0127] A 1 mm magnetic wire (KMK-20E manufactured by Hitachi Metals) was used to prepare a spiral coil as a test piece by the method according to JIS C3216-1 and 6. Next, the spiral coil was preheated by heating it at 150°C for 120 minutes and cooled to room temperature. The spiral coils were quietly immersed in the insulating resin composition (X), lifted after standing for 1 minute, and hung at a suitable interval in the heating furnace. The coils were heated for a specified time to cure the insulating resin composition (X). The heating conditions were set at 170°C for 2 hours. For the spiral coil obtained by heat curing, a 3-point bending test was performed using an autograph (strength testing machine). The evaluation results are shown in the "Strength" column of Table 1. In this evaluation, the fixing force is preferably 100N or more, and the case where the fixing force is 100N or more is recorded as +, the case where the fixing force is less than 100N is recorded as -, and the case where the fixing force is a value exceeding 120N is recorded as ++.
[0128] 3.2.4. Block solidification state
[0129] Ready to simulate Figure 2 The sample of the stator 19 shown was immersed and cured in the insulating resin composition (X) described in Table 1, and the thickness of the block-shaped cured product formed on the lower side of the wound coil part (coil end) and the insulator was measured. The evaluation results are shown in the "Ice Pillar" column of Table 1. In this evaluation, based on the need for removal processing, a thickness of more than 10 mm that requires cutting and grinding is recorded as -, a thickness of more than 5 mm but less than 10 mm that does not require cutting but requires grinding is recorded as -, a thickness of more than 2 mm but less than 5 mm that requires grinding depending on the location is recorded as +, and a thickness of less than 2 mm that does not require grinding is recorded as ++.
[0130] 3.2.5. Touch
[0131] The cured product of the insulating resin composition (X) formed on the surface of the coil or constituent member of the sample of the spiral coil and the simulated stator 19 was touched with a finger, and the touch property was evaluated based on the presence or absence of adhesion of the finger. The evaluation results are shown in the "Touch Property" column of Table 1. In this evaluation, the case where the insulating resin composition (X) adheres to the finger in a liquid or gel state is recorded as -, the case where the stickiness is felt but does not adhere to the finger is recorded as -, and the case where there is no stickiness, dryness, and no adhesion to the finger is recorded as +.
[0132] 3.2.6. Comprehensive evaluation
[0133] In the insulating resin composition (X), in addition to the mechanical strength and the inhibition of the formation of blocky solids, it is also required to have good touch and a biomass degree of 60% or more. The results of such comprehensive evaluation are shown in the "Judgment" column of Table 1. In Table 1, the situation where all these requirements are met is recorded as +, and the situation where any one or more items are not met is recorded as -, showing the final judgment result.
[0134] 3.3. Results and investigation
[0135] As can be seen from Table 1, Examples 1 to 9 have improved touch properties compared to Comparative Examples 5 and 6. This is believed to be because there is no hydroxyl group with a high degree of freedom in the molecule, and the monofunctional vinyl monomers (D-1) and (D-2) having a cyclic skeleton have an effect of suppressing the adsorption of moisture in the air.
[0136] Next, based on the results of Examples 1 to 9 and Comparative Examples 1 to 4, the blending amounts of the monofunctional vinyl monomers (D-1) and (D-2) derived from biomass materials were examined.
[0137] The total amount of the monofunctional vinyl monomers (D-1) and (D-2) is 82 wt% to 84 wt% in Examples 1 and 2, 65 wt% to 78 wt% in Examples 3 to 6, and 60 wt% to 64 wt% in Examples 7 to 9. In Examples 1 to 6, the thickness of the block solidified material is less than 2 mm, which does not need to be removed, and the mechanical strength is also a good value exceeding the target of 100 N. In particular, in Examples 3 to 6, the mechanical strength is more than 120 N. In Examples 7 to 9, the mechanical strength exceeds 100 N, while the thickness of the block solidified material is 2 mm to 5 mm. In Examples 7 to 9, although the removal process of the block solidified material cannot be completely eliminated, the process time and the required processing parts can be greatly reduced, and the effect of improving productivity can be obtained. In Examples 1 to 9, the overall viscosity of the insulating resin composition (X) is 10 mPa·s to 80 mPa·s. In Examples 1 to 9, good results were obtained also regarding the finger touch properties after curing.
[0138] On the other hand, the total amount of the monofunctional vinyl monomer (D-1) and (D-2) in Comparative Examples 1 and 2 exceeds 85wt%. For the thickness of the block solidified product, although it is less than 2mm, which does not need to be removed at all, the necessary value of 100N for mechanical strength is not achieved. Furthermore, in terms of finger touch, a part of it is confirmed to be sticky. It is speculated that this is because the amount of the monofunctional vinyl monomer is extremely large, and a part of it does not contribute to the curing reaction, volatilizes in the curing furnace and fills the furnace, and then adheres to the surface of the coil. In addition, in Comparative Examples 3 and 4 where the total amount of the monofunctional vinyl monomer (D-1) and (D-2) is less than 57wt%, it becomes a + judgment in mechanical strength, and on the other hand, the thickness of the block solidified product exceeds 5mm or 10mm, becoming a - judgment or a - judgment.
[0139] This is because: the monofunctional vinyl monomer (D) helps to improve the deliquescence by reducing the viscosity of the insulating resin composition (X), and has the effect of inhibiting the formation of blocky cured products. On the other hand, due to its low molecular weight and the property of volatilization during curing, it affects the reduction of mechanical strength and touch properties of the cured product (Y). That is, there is a trade-off relationship between the inhibition of blocky cured products and mechanical strength and touch properties that depends on the amount of monofunctional vinyl monomer (D) added. As a result of in-depth research in the present disclosure, it was found that: in order to take these characteristics into account, the amount of monofunctional vinyl monomer (D), especially the amount of monofunctional vinyl monomers (D-1) and (D-2), can be 60wt% to 84wt%, and more preferably 65wt% to 78wt%.
[0140] Next, by comparing Example 3 with Comparative Example 5, the effect of the monofunctional vinyl monomer with a cyclic structure is discussed. Example 3 includes isobornyl methacrylate (D-1) and tetrahydrofurfuryl methacrylate (D-2) having a cyclic skeleton. Comparative Example 5 is an example of using 2-HEMA (D-3) instead of these, and the compounding amount of the monofunctional vinyl monomer (D) is the same. Both of them obtain good results of less than 2mm in the thickness of the block-shaped cured product, but differences are found in mechanical strength and touch. In Example 3 using the monofunctional vinyl monomer with a cyclic structure, the mechanical strength exceeds 120N and the touch is also good. On the other hand, in Comparative Example 5 using 2-HEMA, in addition to the mechanical strength being less than 100N, no improvement in touch is found. This is believed to be because: the molecular skeleton of the monofunctional vinyl monomer having a cyclic skeleton is stronger than that of 2-HEMA having a chain structure; and the monofunctional vinyl monomer having a cyclic skeleton has high hydrophobicity (hydrophilicity is suppressed) because it does not have a hydroxyl group with a high degree of freedom.
[0141] Next, by comparing Example 3 with Comparative Examples 7 and 8, the effect of using two monofunctional vinyl monomers having a cyclic structure in combination was examined. Example 3 contains both isobornyl methacrylate (D-1) and tetrahydrofurfuryl methacrylate (D-2) having a cyclic skeleton. Comparative Examples 7 and 8 contain only one of isobornyl methacrylate (D-1) or tetrahydrofurfuryl methacrylate (D-2). In Example 3, the mechanical strength exceeded 100N, which was a good result. In contrast, in Comparative Examples 7 and 8, although it was small, it was obviously less than 100N. It is believed that this is because: in the case of isobornyl methacrylate (D-1) alone, the bulky isobornyl skeleton hinders the cross-linking structure and the necessary mechanical strength cannot be obtained. On the other hand, it is believed that: in the case of tetrahydrofurfuryl methacrylate (D-2) alone, the strength is lower than that of the isobornyl skeleton, so the necessary mechanical strength cannot be obtained.
[0142] As described above, in the insulating resin composition (X), since the (C) multifunctional vinyl monomer and the (D) multifunctional vinyl monomer use plant-derived biomass materials as raw materials, the environmental load reduction effect is high compared with the insulating resin composed of raw materials derived from petroleum. In addition, the insulating resin composition (X) in the present disclosure can obtain biomass labeling certification (containing 10% or more of biomass materials) by the state or third-party agency, etc., depending on its blending ratio, and can contribute to the formation of a recycling-oriented society.
[0143] In addition, the monofunctional vinyl monomer (D) reduces the viscosity of the insulating resin composition (X), thereby improving the deliquescence of the insulating resin composition (X) when the coil is pulled out of the dipping tank. This prevents the excess insulating resin composition (X) from adhering to the inside of the coil and the constituent members, thereby achieving the effect of suppressing the formation of block-like cured products.
[0144] Moreover, in the monofunctional vinyl monomer (D) contained in the insulating resin composition (X), the vinyl monomer (D-1) having an isobornyl skeleton and the vinyl monomer (D-1) having a cyclic ether skeleton have excellent heat resistance and strength compared with the vinyl monomer having a chain skeleton because they contain a cyclic skeleton in the molecule. As described above, the addition of a reactive diluent is effective for reducing the viscosity of the insulating resin, but in the case of a monofunctional monomer having a chain structure and a small molecular weight, if a large amount is added to achieve the required viscosity, the heat resistance and mechanical strength of the cured product are reduced. In contrast, in the case of the vinyl monomer (D-1) having an isobornyl skeleton and the vinyl monomer (D-1) having a cyclic ether skeleton used in the present disclosure, due to the effect of the cyclic structure in the molecule, the thermal and mechanical properties are excellent compared with the monomer having a chain structure. Therefore, even if these monomers are added in large quantities, the heat resistance and strength properties of the cured product (Y) will not be reduced, and the effect of improving the heat resistance and strength properties is obtained.
[0145] Furthermore, the vinyl monomer (D-1) having an isobornyl skeleton and the vinyl monomer (D-1) having a cyclic ether skeleton do not have a hydroxyl group with a high degree of freedom in the molecule, and therefore have a lower hydrophilicity than 2-HEMA used as a reactive diluent. That is, since the affinity with moisture in the air is low, the insulating resin composition (X) is prevented from reattaching to the surface of the cured product (Y), and the surface touchability is improved.
[0146] In the present disclosure, the vinyl monomer (D-1) having an isobornyl skeleton and the vinyl monomer (D-1) having a cyclic ether skeleton are biomass materials, and they are contained in the monofunctional vinyl monomer (D) as a main component in an amount of about 60 wt% to 84 wt%. Therefore, the biomass degree of the insulating resin composition (X) is 60% or more and 84% or less due to the blending amount of the vinyl monomer (D-1) having an isobornyl skeleton and the vinyl monomer (D-1) having a cyclic ether skeleton.
[0147] Therefore, due to the above-mentioned effects, an insulating resin composition (X) is provided in which a biomass material is used as a raw material and the surface touch property of a cured product is further improved.
[0148] It should be noted that the scope of the present disclosure is not limited to the examples described above, but should be defined by the patent claims. The scope of the present disclosure includes all changes in the meaning equivalent to the patent claims. In addition, the scope of the present disclosure also includes all changes in the scope equivalent to the patent claims.
[0149] Industrial Applicability
[0150] The rotating machine of the present disclosure can be applied to the hoisting machine of a rope elevator. The winding coil of the present disclosure can be applied to the rotating machine. The insulating resin composition and its cured product of the present disclosure can be applied to the insulation and mechanical strength of the coil.
[0151] Description of Reference Numerals
[0152] 1 coil, 2 insulating resin, 3 volatile reactive diluent, 4 water, 5 film, 10 winch, 11 rotating part, 12 brake part, 13 motor part, 14 sheave, 15 rotor, 16 brake disc, 17 rotating shaft, 18 frame, 19 stator, 20 iron core, 21 winding wire, 22 insulator
Claims
1. An insulating resin composition, comprising: A thermosetting resin having both an epoxy group and a meth(acryloyl) group, Free radical polymerization initiators and curing agents for epoxy groups, Multifunctional vinyl monomers made from biomass materials, and Monofunctional vinyl monomers made from biomass materials. The monofunctional vinyl monomer includes both a vinyl monomer having an isobornyl skeleton and a vinyl monomer having a cyclic ether skeleton of a saturated hydrocarbon. The biomass degree is 60% or more and 84% or less.
2. The insulating resin composition according to claim 1, wherein The viscosity is 10 mPa·s or more and 80 mPa·s or less. 3 . A cured product obtained by curing the insulating resin composition according to claim 1 or 2 . 4 . A wound coil impregnated with the insulating resin composition according to claim 1 .
5. A rotating machine used in a hoisting machine for driving a car of a rope-type elevator, comprising: A stator having the wound coil according to claim 4 is used.