Modified ethylene-vinyl alcohol copolymer composition, particles, multilayer structure, method for producing modified ethylene-vinyl alcohol copolymer composition, and method for producing multilayer structure

By adding a trace amount of titanium compound to the modified EVOH resin, the problems of reduced productivity and resin instability caused by thermal deterioration are solved, and the thermal stability and softness of the modified EVOH resin are improved.

CN118765305APending Publication Date: 2024-10-11MITSUBISHI CHEM CORP

Patent Information

Application Number
CN202380023834.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing modified EVOH resins suffer from thermal deterioration in highly functional molding equipment, resulting in reduced productivity, and have problems with coloring and insufficient flexibility.

Method used

A specific trace amount of a titanium compound is added to the modified EVOH resin, and a modified EVOH resin composition is formed through a melt mixing process to suppress thermal degradation and improve the thermal stability of the resin.

Benefits of technology

It effectively suppresses thermal deterioration during melt molding, improves the thermal stability and softness of the resin, reduces the decrease in productivity, and avoids coloring problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012002720000061
    Figure BDA0005012002720000061
  • Figure BDA0005012002720000211
    Figure BDA0005012002720000211
Patent Text Reader

Abstract

Provided is an ethylene-vinyl alcohol copolymer composition in which thermal deterioration during melt molding is suppressed. A modified ethylene-vinyl alcohol copolymer composition containing a modified ethylene-vinyl alcohol copolymer containing an aliphatic polyester unit and a titanium compound, the content of the titanium compound in terms of metal is 0.001 ppm or more and less than 5 ppm relative to the unit mass of the modified ethylene-vinyl alcohol copolymer composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a modified ethylene-vinyl alcohol copolymer composition containing an aliphatic polyester unit, a particle, a multilayer structure, a method for producing the modified ethylene-vinyl alcohol copolymer composition, and a method for producing the multilayer structure. Background Art

[0002] Ethylene-vinyl alcohol copolymers (hereinafter sometimes referred to as "EVOH resins") are excellent in transparency, barrier properties to gases such as oxygen, aroma retention, solvent resistance, oil resistance, mechanical strength, etc., and are formed into films, sheets, bottles, etc., and are widely used as various packaging materials such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, and pesticide packaging materials.

[0003] However, EVOH resin has a relatively active hydroxyl group in the molecule, so it tends to be easily degraded by heat, and is prone to coloring during melt molding. In addition, EVOH resin is a hard and brittle resin and lacks flexibility.

[0004] To address the above problems, for example, Patent Document 1 describes a modified EVOH resin containing an aliphatic polyester unit, wherein the yellowness index (YI) value of the molded article thereof is set to a specific value or less, thereby suppressing deterioration and coloration after thermoforming.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2019 / 163379 Summary of the invention

[0008] Problems to be solved by the invention

[0009] However, although the modified EVOH resin described in the above-mentioned Patent Document 1 can suppress coloration, in recent years, with the diversification of the shapes of feed modules / molds in molding devices, the thinning of multilayer structures in final products, the increase in the number of layers and other requirements for various high functions, there is a tendency for the resin to thermally deteriorate and the productivity of the product to decrease in the molding devices that have become complicated due to the high functions, and further improvement is required.

[0010] The present invention provides a modified EVOH resin composition in which thermal degradation during melt molding is suppressed.

[0011] Methods for solving problems

[0012] However, in view of the above circumstances, the present inventors have found that a modified EVOH resin composition in which thermal degradation during melt molding is suppressed can be obtained by adding a specific trace amount of a titanium compound to a modified EVOH resin containing an aliphatic polyester structural unit.

[0013] That is, the present invention has the following aspects.

[0014] [1] A modified EVOH resin composition comprising a modified EVOH resin containing an aliphatic polyester structural unit and a titanium compound,

[0015] The metal-equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the unit mass of the modified EVOH resin composition.

[0016] [2] The modified EVOH resin composition according to [1], wherein the modification ratio of the aliphatic polyester structural unit in the modified EVOH resin is 0.1 to 30 mol%.

[0017] [3] The modified EVOH resin composition according to [1] or [2], wherein the average chain length of the aliphatic polyester structural units contained in the modified EVOH resin is 1.5 to 3.0.

[0018] [4] The modified EVOH resin composition according to any one of [1] to [3], wherein the aliphatic polyester structural unit is a lactone ring-opening polymer.

[0019] [5] A pellet comprising the modified EVOH resin composition according to any one of [1] to [4].

[0020] [6] A multilayer structure having at least one layer composed of the modified EVOH resin composition according to any one of [1] to [4].

[0021] [7] A method for producing a modified EVOH resin composition, which is a method for producing the modified EVOH resin composition described in any one of [1] to [4],

[0022] The method comprises the step of melt-mixing a composition raw material containing the modified EVOH resin and a titanium compound.

[0023] [8] A method for producing a multilayer structure, which is a method for producing the multilayer structure described in [6],

[0024] The method comprises the step of melt-molding a layer composed of the modified EVOH resin composition.

[0025] Effects of the Invention

[0026] Since the modified EVOH resin composition of the present invention is excellent in thermal stability, thermal degradation of the modified EVOH resin during melt molding can be suppressed. DETAILED DESCRIPTION

[0027] Hereinafter, the present invention will be described in further detail based on embodiments of the present invention, but the present invention is not limited to these embodiments.

[0028] It should be noted that in the present invention, when expressed as "X to Y" (X, Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", and also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0029] In addition, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y".

[0030] <EVOH resin composition>

[0031] A modified EVOH resin composition according to one embodiment of the present invention (hereinafter referred to as "the present modified EVOH resin composition") contains a modified EVOH resin including an aliphatic polyester unit as a main component and contains a specific trace amount of a titanium compound.

[0032] That is, in the modified EVOH resin composition, the base resin is a modified EVOH resin, and the content of the modified EVOH resin in the modified EVOH resin composition is usually 70% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0033] Hereinafter, each component will be described.

[0034] 〔Modified EVOH resin〕

[0035] The modified EVOH resin contains an aliphatic polyester structural unit. In order to ensure gas barrier properties and flexibility, the aliphatic polyester structural unit is preferably bonded to the side chain of the EVOH resin, that is, the aliphatic polyester structural unit is grafted onto the EVOH resin.

[0036] In view of the simplicity of reaction, oozing out, poor adhesion, less evaporation during melt molding, and less pollution to the working environment, it is preferred that the aliphatic polyester structural unit is a lactone ring-opening polymer. Such a modified EVOH resin can be obtained, for example, by a lactone ring-opening polymerization reaction and a grafting reaction in the presence of an EVOH resin.

[0037] Hereinafter, the modified EVOH resin will be described in detail.

[0038] [EVOH resin]

[0039] The EVOH resin used as a raw material of the modified EVOH resin is generally a resin obtained by saponifying an ethylene-vinyl ester copolymer which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.

[0040] As the vinyl ester monomer, vinyl acetate can be used representatively from the aspects of market availability and good impurity treatment efficiency during production. As other vinyl ester monomers other than vinyl acetate, for example, aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate can be mentioned. Generally, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms are used. These are generally used alone, but multiple types may be used simultaneously as needed.

[0041] As the polymerization method for copolymerizing the above-mentioned ethylene and vinyl ester monomers, any known polymerization method such as solution polymerization, suspension polymerization, emulsion polymerization, etc. can be used, but solution polymerization using methanol as a solvent is generally used. In addition, the saponification of the obtained ethylene-vinyl ester copolymer can also be carried out using a known method.

[0042] The EVOH resin produced in this manner mainly contains structural units derived from ethylene and vinyl alcohol, and also contains a certain amount of vinyl ester structural units that remain without being saponified.

[0043] The content of the ethylene structural unit in the EVOH resin is usually 20 to 60 mol%, preferably 25 to 50 mol%, and particularly preferably 25 to 35 mol%. The content of the ethylene structural unit can be controlled by the ethylene pressure when the vinyl ester monomer and ethylene are copolymerized. When the content is too low, the gas barrier properties and melt moldability under high humidity tend to decrease, while when it is too high, the gas barrier properties tend to decrease.

[0044] It should be noted that the content of the ethylene structural unit can be measured based on ISO14663.

[0045] The saponification degree of the EVOH resin is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. The saponification degree can be controlled by the amount of a saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) when saponifying the ethylene-vinyl ester copolymer, the temperature, the time, etc. When the saponification degree is too low, there is a tendency for gas barrier properties, thermal stability, moisture resistance, etc. to decrease.

[0046] The saponification degree of the EVOH resin can be measured in accordance with JIS K6726 (wherein the EVOH resin is used in the form of a solution uniformly dissolved in a water / methanol solvent).

[0047] The melt flow rate (MFR) (210°C, load 2160g) of the EVOH resin is usually 0.5 to 100g / 10min, preferably 1 to 50g / 10min, and particularly preferably 3 to 35g / 10min. When the MFR is too large, the stability during film formation tends to be impaired, and when it is too small, the viscosity tends to become too high and melt extrusion tends to become difficult.

[0048] The MFR is an index of the degree of polymerization of the EVOH resin, and can be adjusted by the amount of the polymerization initiator and the amount of the solvent when ethylene and the vinyl ester monomer are copolymerized.

[0049] Furthermore, the EVOH resin may further contain a structural unit derived from the following comonomer (for example, 10 mol % or less of the EVOH resin) within a range not impairing the effects of the present invention.

[0050] Examples of the comonomer include olefins such as propylene, 1-butene, and isobutylene; hydroxyl-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol; and derivatives thereof such as esters and acylates; hydroxyalkyl vinylides such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane; Methylpropane, 1,3-dibutyryloxy-2-methylenepropane and other hydroxyalkyl vinylene esters; acrylic acid, methacrylic acid, crotonic acid, phthalic acid (anhydride), maleic acid (anhydride), itaconic acid (anhydride) and other unsaturated acids or their salts or mono- or di-alkyl esters with alkyl carbon number of 1 to 18; acrylamide, N-alkyl acrylamide with alkyl carbon number of 1 to 18, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salt, acrylamidopropyl dimethylamine or Acrylic amides such as its acid salt or quaternary salt thereof; methacrylamide, N-alkyl methacrylamide with an alkyl group having 1 to 18 carbon atoms, N,N-dimethyl methacrylamide, 2-methacrylamide propanesulfonic acid or its salt, methacrylamide propyl dimethylamine or its acid salt or quaternary salt thereof; N-vinyl amides such as N-vinyl pyrrolidone, N-vinyl formamide, N-vinyl acetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; 8, alkyl vinyl ethers, hydroxyalkyl vinyl ethers, alkoxyalkyl vinyl ethers and other vinyl ethers; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide, etc.; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; comonomers such as trimethyl-(3-acrylamide-3-dimethylpropyl)-ammonium chloride and acrylamide-2-methylpropanesulfonic acid. These can be used alone or in combination of two or more.

[0051] Among them, hydroxyl-containing α-olefins are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the above-mentioned hydroxyl-containing α-olefins are copolymerized, the obtained EVOH resin has a primary hydroxyl group in the side chain. From the perspective of maintaining gas barrier properties and improving secondary moldability, such EVOH resins with primary hydroxyl groups in the side chain, especially EVOH resins with a 1,2-diol structure in the side chain, are preferred.

[0052] When the EVOH resin has a primary hydroxyl group in the side chain, the content of the structural unit derived from the monomer having the primary hydroxyl group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, particularly preferably 1 to 10 mol % of the EVOH resin.

[0053] [Lactones]

[0054] As described above, lactones form aliphatic polyester structural units by ring-opening polymerization, which are grafted with EVOH resin to obtain modified EVOH resin. Such lactones are not particularly limited as long as they have 3 to 10 carbon atoms constituting the lactone ring.

[0055] When the lactone has no substituent, it is represented by the following general formula (1).

[0056] [Chemistry 1]

[0057]

[0058] In the above general formula (1), n ​​is an integer of 2 to 9, preferably 4 to 5. In addition, the alkylene chain (-(CH2) n Any carbon atom contained in the group (-) may have a substituent such as a lower alkyl group having about 1 to 8 carbon atoms, a lower alkoxy group having about 1 to 8 carbon atoms, a cycloalkyl group, a phenyl group, an aralkyl group, etc. The number of such substituents may be one or more.

[0059] Specific examples of the lactones include β-propiolactones, γ-butyrolactones, ε-caprolactones, and δ-valerolactones.

[0060] Examples of the β-propiolactones include β-propiolactone and dimethylpropiolactone.

[0061] Examples of the γ-butyrolactones include γ-butyrolactone, γ-valerolactone, γ-caprolactone, γ-decanolactone, γ-laurolactone, γ-palmitolactone, γ-stearoyl lactone, crotonyl lactone, α-angelica lactone, and β-angelica lactone.

[0062] Examples of the above-mentioned ε-caprolactones include monoalkyl-ε-caprolactones such as ε-caprolactone, monomethyl-ε-caprolactone, monoethyl-ε-caprolactone, monodecyl-ε-caprolactone, and monopropyl-ε-caprolactone; dialkyl-ε-caprolactones having two alkyl groups substituted on carbon atoms other than the ε position; trialkyl-ε-caprolactones having three alkyl groups substituted on carbon atoms other than the ε position; alkoxy-ε-caprolactones such as ethoxy-ε-caprolactone; cycloalkyl lactones such as cyclohexyl-ε-caprolactone; aralkyl-ε-caprolactones such as benzyl-ε-caprolactone; aryl-ε-caprolactones such as phenyl-ε-caprolactone, and the like.

[0063] Examples of the δ-valerolactones include 5-valerolactone, 3-methyl-5-valerolactone, 3,3-dimethyl-5-valerolactone, 2-methyl-5-valerolactone, and 3-ethyl-5-valerolactone.

[0064] These lactones may be used alone or in combination of two or more. Among them, ε-caprolactone or δ-valerolactone is preferred from the aspect of reactivity, ε-caprolactone is more preferred from the aspect of low cost and easy availability, and ε-caprolactone is particularly preferred.

[0065] [Method for producing modified EVOH resin]

[0066] The modified EVOH resin is obtained by subjecting lactone to ring-opening polymerization in the presence of the EVOH resin, and grafting the aliphatic polyester structural unit obtained by the ring-opening polymerization onto the hydroxyl group of the EVOH resin as the starting terminal.

[0067] The ring-opening polymerization reaction and grafting reaction of the lactones are usually carried out in a molten state of the EVOH resin, and examples thereof include a method in which the EVOH resin, lactones, catalyst and other materials are heated and stirred in a stirring tank type manufacturing device with stirring blades, an extruder, etc. Among them, the method using an extruder is preferred.

[0068] Examples of the extruder include single-screw extruders, twin-screw extruders, Banbury mixers, kneaders, and Brabender extruders (e.g., TEX series manufactured by Nippon Steel Works, Ltd., HYPERKTX series manufactured by Kobe Steel, Ltd., TEM series manufactured by Shibaura Machine Co., Ltd., and KRC kneader series manufactured by Kurimoto Iron Works Co., Ltd.). An extruder that can continuously carry out a grafting reaction of EVOH resin by melt kneading (also referred to as a continuous type) may also be used.

[0069] The continuous method is a method of sequentially feeding various raw materials into an extruder, and reacting them at a predetermined temperature while stirring to continuously synthesize a resin composition, wherein the feeding of the raw materials and the discharge of the resin composition are carried out simultaneously.

[0070] The amount of lactone used relative to the above-mentioned EVOH resin can be appropriately selected so as to include the desired content of aliphatic polyester units in the EVOH resin, and is generally 1 to 200 parts by mass, preferably 10 to 150 parts by mass, and particularly preferably 20 to 100 parts by mass relative to 100 parts by mass of the EVOH resin. If the amount of lactone used is too small, there is a tendency for the flexibility to decrease, and on the other hand, if the amount used is too large, there is a tendency for the gas barrier properties to decrease.

[0071] As the catalyst, a conventionally known ring-opening polymerization catalyst for lactones can be used, and examples thereof include titanium compounds and tin compounds.

[0072] As the titanium compound, for example, alkoxytitanium such as tetra-n-butoxytitanium, tetraisobutoxytitanium, and tetraisopropoxytitanium can be cited. As the tin compound, for example, tin alkoxides such as dibutyl dibutoxytin, 2-ethylhexanoic acid tin, dibutyl tin diacetate and other tin ester compounds can be cited. These can be used alone or in combination of two or more. Among them, tin compounds are preferred, tin ester compounds are more preferred, and 2-ethylhexanoic acid tin is particularly preferred.

[0073] The amount of the catalyst used is usually 0.01 to 10 parts by mass, preferably 0.05 to 8 parts by mass, and particularly preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the lactone. If the amount of the catalyst used is too small or too large, the modification rate tends to decrease.

[0074] The reaction temperature in the ring-opening polymerization reaction and the grafting reaction is usually 50 to 250° C., preferably 100 to 240° C., and more preferably 150 to 230° C., which is a molten state. If the reaction temperature is too high, the modified EVOH resin tends to be thermally degraded. On the other hand, if the reaction temperature is too low, the grafting reaction tends not to proceed.

[0075] The reaction time in the ring-opening polymerization reaction and the grafting reaction is usually 1 second to 1.5 hours, preferably 3 seconds to 1.25 hours, more preferably 5 seconds to 1 hour, and particularly preferably 7 seconds to 45 minutes. If the reaction time is too long, the extreme viscosity of the modified EVOH resin increases due to thermal degradation of the modified EVOH resin and thermal degradation products are produced in the modified EVOH resin, so that there is a tendency to produce gel during film production of films, etc. On the other hand, if the reaction time is too short, the grafting reaction of the EVOH resin does not proceed, and there is a tendency for the unmodified EVOH resin to increase.

[0076] It should be noted that, in order to prevent the deterioration of the EVOH resin, the ring-opening polymerization reaction and the grafting reaction are preferably carried out under a nitrogen flow.

[0077] In addition, after the reaction, in order to prevent odor, it is also preferred to remove unreacted monomers. As a method for removing unreacted monomers, for example, a method of immersing in a solution dissolving unreacted monomers, a method of removing under reduced pressure, etc. can be cited. From the viewpoint of production efficiency, a method of removing under reduced pressure is preferred. As the conditions for the above-mentioned removal under reduced pressure, it is sufficient to perform the removal under a pressure of 100 to 101200 Pa for 1 second to 10 hours at the same set temperature as the reaction temperature.

[0078] The modified EVOH resin is obtained in this way, and the content of the EVOH resin structural unit forming the backbone of the obtained modified EVOH resin is usually 40 to 99% by mass, preferably 45 to 95% by mass, and particularly preferably 50 to 90% by mass. If the content of the EVOH resin structural unit in the modified EVOH resin is too high, there is a tendency for the flexibility to decrease, while on the other hand, if the content of the EVOH resin structural unit is too low, there is a tendency for the gas barrier properties to decrease.

[0079] The content of the aliphatic polyester structural unit grafted onto the EVOH resin is usually 1 to 60% by mass, preferably 5 to 55% by mass, and particularly preferably 10 to 50% by mass.

[0080] The modification rate of the aliphatic polyester structural unit in the modified EVOH resin is preferably 0.1 to 30 mol%, more preferably 1 to 20 mol%, and particularly preferably 5 to 15 mol%. The modification rate refers to the proportion of the EVOH resin structural unit grafted onto the aliphatic polyester. If the modification rate of the modified EVOH resin is too low, there is a tendency for the softness to decrease. On the other hand, if the modification rate of the modified EVOH resin is too high, there is a tendency for the gas barrier properties to decrease.

[0081] The average chain length of the aliphatic polyester structural unit grafted onto the EVOH resin is preferably 1.5 to 3.0, more preferably 1.6 to 2.8, and particularly preferably 1.7 to 2.5. If the average chain length of the aliphatic polyester unit is too long, there is a tendency for the gas barrier properties to decrease. It should be noted that the average chain length of the aliphatic polyester structural unit represents the degree of polymerization during the ring-opening polymerization of the lactone.

[0082] The content of the EVOH resin structural unit in the modified EVOH resin, the content of the grafted aliphatic polyester unit, the modification rate of the modified EVOH resin and the average chain length of the aliphatic polyester unit can be calculated according to 1 It was calculated based on the results of H-NMR measurement.

[0083] The number average molecular weight of the modified EVOH resin is usually 10000 to 300000, preferably 12500 to 200000, and particularly preferably 15000 to 100000. If the number average molecular weight of the modified EVOH resin is too high, the gas barrier properties tend to be reduced, while if the number average molecular weight of the modified EVOH resin is too low, the flexibility tends to be reduced.

[0084] In addition, the said number average molecular weight is the value measured by gel permeation chromatography (GPC) using standard polystyrene.

[0085] The melting point of the modified EVOH resin is usually 40 to 200° C., preferably 60 to 180° C., more preferably 80 to 160° C., and particularly preferably 100 to 140° C. If the melting point of the modified EVOH resin is too high, the flexibility tends to decrease, while if the melting point of the modified EVOH resin is too low, the gas barrier properties tend to decrease.

[0086] It should be noted that the melting point of the modified EVOH resin can be measured using a differential scanning calorimeter.

[0087] Generally, by grafting aliphatic polyester structural units, intermolecular forces such as hydrogen bonds between hydroxyl groups in the backbone EVOH resin are weakened. Therefore, if the modification rate of the modified EVOH resin increases, the melting point of the modified EVOH resin tends to decrease.

[0088] 〔Titanium compounds〕

[0089] Examples of the titanium compound include inorganic titanium compounds and organic titanium compounds. It should be noted that the titanium compound may be used alone or in combination of two or more. Among them, inorganic titanium compounds are preferred.

[0090] Examples of the inorganic titanium compound include titanium oxide, titanium hydroxide, titanium chloride, and inorganic titanium salts.

[0091] Examples of the titanium oxide include titanium (II) oxide, titanium (III) oxide, titanium (IV) oxide, and titanous oxide.

[0092] Examples of the titanium hydroxide include titanium hydroxide and titanium hydroxide.

[0093] Examples of the titanium chloride include titanous chloride and titanium chloride.

[0094] Examples of the inorganic salt of titanium include titanium phosphate and titanium sulfate.

[0095] Among them, titanium oxide is preferred, titanium (IV) oxide is more preferred, and rutile titanium (IV) oxide is particularly preferred.

[0096] Examples of the organic titanium compound include titanium acetate, titanium butyrate, titanium stearate and other titanium carboxylates.

[0097] It should be noted that the titanium compound may exist in the modified EVOH resin composition in the form of a titanium compound, or in an ionized state or in the form of a complex formed by interaction with the modified EVOH resin or other ligands.

[0098] The average particle size of the titanium compound is usually 0.001 to 100 μm, preferably 0.01 to 50 μm, and more preferably 0.015 to 20 μm. When the average particle size of the titanium compound is within the above range, thermal deterioration tends to be suppressed.

[0099] The metal conversion content of the above-mentioned titanium compound is 0.001ppm or more and less than 5ppm relative to the unit mass of the modified EVOH resin composition. It is preferably 0.01 to 3ppm, more preferably 0.03 to 1ppm, and particularly preferably 0.05 to 0.5ppm. By setting the content of the titanium compound to the above range, the degradation caused by heat during melt molding can be suppressed. In addition, if the content of the titanium compound is too small, the effect of suppressing the degradation caused by heat is reduced, and if the content is too much, thermal decomposition of the modified EVOH resin is likely to occur, and it is easy to color.

[0100] Generally, modified EVOH resin deteriorates due to heat. This is believed to be because the modified EVOH resin deteriorates due to heat and generates free radicals, which dehydrate the hydroxyl groups of the modified EVOH resin and generate double bonds in the main chain of the modified EVOH resin. This site becomes the starting point of the reaction, further promoting dehydration and forming a conjugated polyene structure in the main chain of the modified EVOH resin.

[0101] On the other hand, the modified EVOH resin composition of the present invention can suppress thermal degradation of the modified EVOH resin by containing a specific trace amount of a titanium compound.

[0102] Generally, when a titanium compound is contained in an EVOH resin composition, it is believed that the EVOH resin composition is thermally decomposed by titanium ions, and therefore it is common knowledge for those skilled in the art to avoid using titanium compounds. However, in the present invention, contrary to such common knowledge, it is found that a modified EVOH resin composition with suppressed thermal degradation can be obtained by using a specific trace amount of a titanium compound.

[0103] That is, it is presumed that titanium is stable as a tetravalent ion and coordinates to the double bonds of the main chain of the modified EVOH resin as described above even in a trace amount to form a chelate or the like, thereby stabilizing and suppressing the formation of a polyene structure.

[0104] On the other hand, if the content of the titanium compound is too large, it is considered that the modified EVOH resin is thermally decomposed by the titanium compound.

[0105] [Other thermoplastic resins]

[0106] The modified EVOH resin composition may contain a thermoplastic resin other than the modified EVOH resin within a range that does not impair the effects of the present invention (e.g., generally 30% by mass or less, preferably 20% by mass or less, particularly preferably 10% by mass or less of the modified EVOH resin composition).

[0107] As other thermoplastic resins, known thermoplastic resins can be used, for example, EVOH resin, polyester resin, polystyrene resin, polyvinyl chloride resin, polycarbonate resin, ionomer resin, polyvinylidene chloride, polyester elastomer, polyurethane elastomer, chlorinated polyethylene, chlorinated polypropylene, etc. These can be used alone or in combination of two or more.

[0108] [Other compounding ingredients]

[0109] In addition, the modified EVOH resin composition may contain compounding agents that are usually added to EVOH resins within a range that does not impair the effects of the present invention. As the above-mentioned compounding agents, for example, inorganic complex salts (such as hydrotalcite), plasticizers (such as aliphatic polyols such as ethylene glycol, glycerol, hexylene glycol, etc.), oxygen absorbers [such as inorganic oxygen absorbers such as aluminum powder and potassium sulfite; ascorbic acid, further its fatty acid esters, metal salts, etc., gallic acid, polyphenols such as hydroxyl phenolic resins, terpene compounds, blends of tertiary hydrogen-containing resins and transition metals (such as a combination of polypropylene and cobalt), blends of resins containing carbon-carbon unsaturated bonds and transition metals (such as polybutadiene and [combination of cobalt, photo-oxidative degradable resin (e.g., polyketone), anthraquinone polymer (e.g., polyvinyl anthraquinone), etc., and the like ...

[0110] [Method for producing EVOH resin composition]

[0111] The modified EVOH resin composition can be manufactured, for example, by mixing the modified EVOH resin and the titanium compound by a known method such as dry blending, melt mixing, solution mixing, impregnation, etc., wherein it is preferably manufactured by a process of melt mixing the composition raw materials containing the modified EVOH resin and the titanium compound. In addition, these manufacturing methods can also be arbitrarily combined.

[0112] Examples of the dry blending method include (i) a method of dry blending a pelletized modified EVOH resin and a titanium compound using a tumbler.

[0113] Examples of the melt mixing method include: (ii) a method of melt kneading a dry blend obtained by dry-blending a pelletized modified EVOH resin and a titanium compound; and (iii) a method of adding a titanium compound to a molten modified EVOH resin and melt kneading the mixture.

[0114] Examples of the solution mixing method include: (iv) a method in which a solution is prepared using a commercially available modified EVOH resin, a titanium compound is added to the solution, the solution is solidified and formed, and then the solution is separated from the solid by a known method and dried; (v) a method in which, during the manufacturing process of the modified EVOH resin, a titanium compound is added to an ethylene-vinyl ester copolymer solution before saponification or a uniform solution of EVOH resin (water / alcohol solution, etc.), the solution is solidified and formed, and then the solution is separated from the solid by a known method and dried.

[0115] Examples of the impregnation method include (vi) a method in which a granular modified EVOH resin is brought into contact with an aqueous solution containing a titanium compound to allow the modified EVOH resin to contain the titanium compound and then dry the solution.

[0116] As the aqueous solution containing a titanium compound, an aqueous solution of a titanium compound or an aqueous solution obtained by immersing a titanium compound in water containing various chemicals to dissolve titanium ions can be used.

[0117] In the above-mentioned impregnation method, the content of the titanium compound (in terms of metal) can be controlled by the concentration of the titanium compound in the aqueous solution in which the modified EVOH resin is impregnated, the impregnation temperature, the impregnation time, and the like.

[0118] The immersion temperature and immersion time are usually 0.5 to 48 hours, preferably 1 to 36 hours, and the immersion temperature is usually 10 to 40°C, preferably 20 to 35°C.

[0119] As the drying method in each of the above-mentioned production methods, various drying methods can be adopted, and any of static drying and fluidized drying can be adopted. In addition, these methods can also be combined.

[0120] As described above, in the present invention, the above different methods can be combined. Among them, from the perspective of obtaining a resin composition with higher productivity and the effect of the present invention, the melt mixing method is preferred, and the method (ii) is particularly preferred. In addition, when using the above other thermoplastic resins and other compounding agents, they can be compounded by conventional methods according to the above manufacturing method.

[0121] The modified EVOH resin composition obtained by the above-mentioned production methods may be in any shape, but is preferably in the form of pellets.

[0122] As the above-mentioned particles, for example, there are spherical, elliptical, cylindrical, cubic, rectangular parallelepiped, etc., usually elliptical or cylindrical, and its size is considered from the perspective of convenience when used as a molding material later. In the case of an elliptical shape, the short diameter is usually 1 to 10 mm, preferably 2 to 6 mm, and more preferably 2.5 to 5.5 mm, and the long diameter is usually 1.5 to 30 mm, preferably 3 to 20 mm, and more preferably 3.5 to 10 mm. In addition, in the case of a cylindrical shape, the diameter of the bottom surface is usually 1 to 6 mm, preferably 2 to 5 mm, and the length is usually 1 to 6 mm, preferably 2 to 5 mm.

[0123] Furthermore, the shape and size of the pelletized modified EVOH resin used in the above-mentioned production methods are also preferably the same.

[0124] The modified EVOH resin composition can suppress thermal degradation during melt molding, and the weight loss rate of the modified EVOH resin composition is usually 9.3% or less, preferably 9.1% or less, and particularly preferably 8.9% or less. The lower limit of the above weight loss rate is as low as possible, but is usually 1%.

[0125] It should be noted that the above-mentioned difference of 0.1% in weight reduction rate manifests as a large difference in yield rate in actual production, and therefore the difference is very large.

[0126] The weight loss rate is a value obtained by measuring the mass of 5 mg of pellets of the modified EVOH resin composition using a thermogravimetric analyzer (Pyris 1TGA manufactured by Perkin Elmer) under nitrogen atmosphere at an air flow rate of 20 mL / min, a temperature of 230° C., and a time of 1 hour, and using the following formula.

[0127] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0128] The water content of the modified EVOH resin composition is usually 0.01 to 0.5% by mass, preferably 0.05 to 0.35% by mass, and particularly preferably 0.1 to 0.3% by mass.

[0129] In addition, the water content of this modified EVOH resin composition is a value measured and calculated by the following method.

[0130] The mass (W1) of the modified EVOH resin composition before drying was weighed with an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and weighed after cooling in the dryer for 30 minutes (W2), and the mass was calculated by the following formula.

[0131] Water content (mass %) = [(W1-W2) / W1] × 100

[0132] In addition, when the modified EVOH resin composition is in the form of pellets, it is also preferred to attach a known lubricant to the surface of the pellets from the perspective of stabilizing the feeding property during melt molding. Examples of lubricants include higher fatty acids having 12 or more carbon atoms (e.g., lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, oleic acid, etc.), higher fatty acid esters (methyl esters, isopropyl esters, butyl esters, octyl esters, etc. of higher fatty acids), higher fatty acid amides (e.g., saturated higher fatty acid amides such as lauramide, myristic acid, palmitic acid, stearic acid, behenic acid amide; unsaturated higher fatty acid amides such as oleamide and erucic acid amide, bis-higher fatty acid amides such as ethylene bisstearamide, ethylene bisoleamide, ethylene biserucic acid amide, ethylene bislauric acid amide, etc.), low molecular weight polyolefins (e.g., low molecular weight polyethylene having a molecular weight of about 500 to 10,000, or low molecular weight polypropylene, etc., or acid-modified products thereof), higher alcohols having 6 or more carbon atoms, ester oligomers, fluoroethylene resins, etc. These compounds may be used alone or in combination of two or more. The content of the lubricant is usually 5% by mass or less, preferably 1% by mass or less, of the modified EVOH resin composition. The lower limit is usually 0% by mass.

[0133] The modified EVOH resin composition thus obtained can be modulated into various forms such as granules, powders, and liquids, and provided as a molding material for various molded products. In particular, in the present invention, when provided as a material for melt molding, there is a tendency to more effectively obtain the effects of the present invention, and therefore it is preferred.

[0134] It should be noted that the modified EVOH resin composition of the present invention also includes a resin composition obtained by mixing a resin other than the modified EVOH resin used in the modified EVOH resin composition of the present invention.

[0135] Examples of the molded product include a multilayer structure having a layer composed of the present modified EVOH resin composition, typified by a single-layer film molded from the present modified EVOH resin composition.

[0136] [Multilayer structure]

[0137] A multilayer structure according to one embodiment of the present invention (hereinafter referred to as "the present multilayer structure") comprises a layer composed of the present modified EVOH resin composition. The layer composed of the present modified EVOH resin composition (hereinafter referred to as "the present modified EVOH resin composition layer") can be further provided with strength, or the present modified EVOH resin composition layer can be protected from the influence of moisture, etc., or other functions can be provided by laminating the layer composed of the present modified EVOH resin composition (hereinafter referred to as "the present modified EVOH resin composition layer") with another substrate having a thermoplastic resin other than the present modified EVOH resin composition as a main component (hereinafter, the resin used for the substrate is sometimes referred to as "substrate resin").

[0138] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and polyolefin resins such as polypropylene resins modified with unsaturated carboxylic acids or The esters thereof include polyolefin resins in a broad sense, such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft-modifying these polyolefins, ionomer resins, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, aromatic or aliphatic polyketones, etc. These may be used alone or in combination of two or more.

[0139] Among them, preferred are polyamide resins, polyolefin resins, polyester resins, and polystyrene resins as hydrophobic resins, and more preferred are polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof.

[0140] When the modified EVOH resin composition layer is a (a1, a2, ...) and the base resin layer is b (b1, b2, ...), the layer structure of the multilayer structure may be any combination of a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, b2 / b1 / a / b1 / a / b1 / b2, etc. In addition, when the regenerated layer obtained by remelting and molding the end portion, defective product, etc. generated in the process of manufacturing the multilayer structure and comprising a mixture of the modified EVOH resin composition and a thermoplastic resin other than the modified EVOH resin composition is R, it may also be b / R / a, b / R / a / b, b / R / a / R / b, b / a / R / a / b, b / R / a / R / a / R / b, etc. The number of layers of the multilayer structure is generally 2 to 15, preferably 3 to 10 in total. In the above-mentioned layer structure, an adhesive resin layer containing an adhesive resin may be interposed between the layers as necessary.

[0141] As the above-mentioned adhesive resin, known substances can be used, as long as they are appropriately selected according to the type of thermoplastic resin used in the substrate resin layer "b". Representative examples include: modified polyolefin polymers containing carboxyl groups obtained by chemically bonding unsaturated carboxylic acids or their anhydrides to polyolefin resins through addition reactions, grafting reactions, etc. As the above-mentioned modified polyolefin polymers containing carboxyl groups, for example, maleic anhydride grafted modified polyethylene, maleic anhydride grafted modified polypropylene, maleic anhydride grafted modified ethylene-propylene (block and random) copolymers, maleic anhydride grafted modified ethylene-ethyl acrylate copolymers, maleic anhydride grafted modified ethylene-vinyl acetate copolymers, maleic anhydride modified polycyclic olefin resins, maleic anhydride grafted modified polyolefin resins, etc. can be listed. They can be used alone or in combination of two or more.

[0142] In the present multilayer structure, when an adhesive resin layer is used between the present modified EVOH resin composition layer and the base resin layer, since the adhesive resin layer is located on both sides of the present modified EVOH resin composition layer, it is preferable to use an adhesive resin with excellent hydrophobicity.

[0143] The above-mentioned base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, nucleating materials, antiblocking agents, waxes, etc. within a range that does not impair the gist of the present invention (e.g., 30% by mass or less, preferably 10% by mass or less relative to the entire resin). These may be used alone or in combination of two or more.

[0144] The lamination of the modified EVOH resin composition layer and the substrate resin layer (including the case where an adhesive resin layer is interposed) can be carried out by a known method. For example, there can be listed: a method of melt-extrusion laminating the substrate resin on a film, sheet, etc. of the modified EVOH resin composition; a method of melt-extrusion laminating the modified EVOH resin composition on the substrate resin layer; a method of co-extruding the modified EVOH resin composition and the substrate resin; a method of dry laminating the modified EVOH resin composition (layer) and the substrate resin (layer) using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, a polyurethane compound, etc.; a method of removing the solvent after applying a solution of the modified EVOH resin composition on the substrate resin, etc. Among these, from the perspective of cost and environment, it is preferred to manufacture by a process of melt-molding the modified EVOH resin composition layer, and specifically, a co-extrusion method is preferred.

[0145] The present multilayer structure can be subjected to (heating) stretching treatment as required. The stretching treatment can be any of uniaxial stretching and biaxial stretching. In the case of biaxial stretching, it can be stretched simultaneously or successively. In addition, as a stretching method, a method with a high stretching ratio such as a roller stretching method, a tenter stretching method, a tubular stretching method, a stretch blow molding method, and a vacuum pressure forming method can be adopted. The stretching temperature is a temperature near the melting point of the multilayer structure, usually 40 to 170°C, preferably selected from the range of about 60 to 160°C. When the stretching temperature is too low, the stretchability becomes poor, and when it is too high, it is difficult to maintain a stable stretched state.

[0146] In addition, the stretched multilayer structure may be heat-fixed for the purpose of imparting dimensional stability. Heat-fixing may be performed in a known manner, for example, by heat-treating the stretched multilayer structure for about 2 to 600 seconds at a temperature of usually 80 to 180° C., preferably 100 to 165° C., while maintaining the stretched multilayer structure in a tensioned state.

[0147] When the present multilayer structure after the stretching treatment is used as a shrink film, in order to impart heat shrinkage, the present multilayer structure after the stretching treatment may be cooled and fixed by blowing cold air instead of the heat setting.

[0148] The thickness of the present multilayer structure (including the stretched multilayer structure), the thickness of the present modified EVOH resin composition layer, the base resin layer and the adhesive resin layer further constituting the multilayer structure cannot be generalized due to the differences in layer constitution, type of base resin, type of adhesive resin, application, packaging method, required physical properties, etc., but the thickness of the present multilayer structure (including the stretched multilayer structure) is usually 10 to 5000 μm, preferably 30 to 3000 μm, and particularly preferably 50 to 2000 μm. The present modified EVOH resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm, the base resin layer is usually 5 to 3000 μm, preferably 10 to 2000 μm, and particularly preferably 20 to 1000 μm, and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0149] Furthermore, regarding the thickness ratio of the modified EVOH resin composition layer to the substrate resin layer in the present multilayer structure (the present modified EVOH resin composition layer / the substrate resin layer), when there are multiple layers, the ratio between the thickest layers is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60. In addition, regarding the thickness ratio of the modified EVOH resin composition layer to the adhesive resin layer in the present multilayer structure (the present modified EVOH resin composition layer / the adhesive resin layer), when there are multiple layers, the ratio between the thickest layers is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10.

[0150] In addition, the present multilayer structure can also be used to obtain a multilayer container in the shape of a cup or a tray. In this case, a deep drawing method is usually used, and specifically, vacuum forming, pressure forming, vacuum pressure forming, plunger-assisted vacuum pressure forming, etc. can be listed. Furthermore, in the case of obtaining a tube or bottle-shaped multilayer container (laminated structure) from a multilayer parison (a hollow tubular preform before blow molding), a blow molding method can be used. Specifically, extrusion blow molding (double-head type, mold moving type, parison moving type, rotary type, accumulator type, horizontal parison type, etc.), cold parison blow molding, injection blow molding, biaxial stretch blow molding (extrusion cold parison biaxial stretch blow molding, injection cold parison biaxial stretch blow molding, injection molding online biaxial stretch blow molding, etc.) can be listed. The obtained laminate may be subjected to heat treatment, cooling treatment, calendaring treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making processing, drawing processing, box processing, tube processing, slitting processing, etc. as necessary.

[0151] The single-layer film formed from the modified EVOH resin composition, the bag composed of the multilayer structure, and the container and cover composed of cups, trays, tubes, bottles, etc. are useful not only as packaging material containers for ordinary foods, but also as packaging material containers for various condiments such as mayonnaise and salad dressing, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, and pharmaceuticals.

[0152] Example

[0153] Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following examples in any way.

[0154] It should be noted that the "portions" in the examples refer to the mass standard unless otherwise specified.

[0155] <Example 1>

[0156] [Manufacturing of modified EVOH resin]

[0157] 100 parts of EVOH resin (ethylene structural unit content 32 mol%, saponification degree 99.8 mol%, MFR 3 g / 10 minutes (210°C, 2160 g)), 47 parts of ε-caprolactone (Placcel M, manufactured by Daicel Corporation) and 1.4 parts of tin 2-ethylhexanoate (NEOSTANN U-28, manufactured by Nitto Chemical Industry Co., Ltd.) (3 parts relative to 100 parts of ε-caprolactone) are put into a twin-screw kneading extruder (TEX30α, manufactured by Nippon Steel Works, Ltd.), conveyed to the melting section with a residence time set to 2 to 3 minutes, and reacted while being melt-kneaded under the following extrusion conditions to obtain pellets of modified EVOH-based resin (modification rate 6.9 mol%, average chain length of aliphatic polyester units 2.3, melting point 121°C).

[0158] [Extrusion conditions]

[0159] Extruder set temperature (°C): C2 / C3 / C4 / C5 / C6 / C7 / C8 / C9 / C10 / C11 / C12 / C13 / C14 / C15 / C16 / D=80 / 80 / 150 / 150 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230 / 230

[0160] It should be noted that the modification rate and the average chain length of the aliphatic polyester unit in the modified EVOH resin can be determined by 1 It was calculated by H-NMR measurement.

[0161] [Determination of Modification Rate and Average Chain Length of Aliphatic Polyester Units]

[0162] (a) 1H-NMR measurement conditions

[0163] Apparatus: Ascend 400 (400 MHz NMR) (manufactured by Bruker)

[0164] Internal standard substance: tetramethylsilane

[0165] Solvent: d6-DMSO

[0166] Determination of polymer concentration: 5 wt% (sample 0.05 g, solvent 1 mL)

[0167] Measurement temperature: 50℃(323K)

[0168] Irradiation pulse: 45° pulse

[0169] Pulse interval: 10sec

[0170] Cumulative times: 16 times

[0171] (b) Attribution of resonance absorption peak

[0172] (I) 0.8~0.9ppm: -CH3 at the end of modified EVOH resin

[0173] (II) 1.0 to 1.9 ppm: -CH2- in the main chain of the modified EVOH resin and -CH2- adjacent to the aliphatic polyester

[0174] (III) 2.0 ppm: -CH3 of residual acetyl group in modified EVOH resin

[0175] (IV) 2.1 to 2.3 ppm: -CH2- adjacent to the carboxyl group of the aliphatic polyester

[0176] (V) 3.3 to 4.0 ppm: -CH- adjacent to -OH of modified EVOH resin and -CH2- adjacent to -OH of aliphatic polyester

[0177] (VI) 4.0 to 4.7 ppm: -OH of modified EVOH resin and aliphatic polyester, and -CH2- adjacent to the ester bond of aliphatic polyester

[0178] (c) Calculation of modification rate and average chain length of aliphatic polyester units

[0179] The integrated values ​​of the resonance absorption peaks of (I) to (VI) are used to establish the simultaneous equations of formulas (i) to (vi), and the graft modification group amount C (mole) and the average chain length n (pieces) of the aliphatic polyester are calculated based on the solutions of the simultaneous equations. Furthermore, the graft modification rate X (mole %) of the aliphatic polyester is calculated based on formula (vii).

[0180] Formula (i) 3×M=[integral value of peak (I)]

[0181] Formula (ii) (2×M)+(2×A)+(4×E)+(2×O)+(6×n+2)×C=[integral value of peak (II)]

[0182] Formula (iii) 3×A=[integral value of peak (III)]

[0183] Formula (vi) 2×n×C=[integral value of peak (IV)]

[0184] Formula (v) O + (2 × C) = [integral value of peak (V)]

[0185] Formula (vi) O + (2 × n-1) × C = [integral value of peak (VI)]

[0186] Formula (vii)X=C / (M+A+O+C+E)×100

[0187] Here, M, A, O, C, n, E, and X represent the following values.

[0188] M: The amount of terminal methyl groups of the modified EVOH resin (mole)

[0189] A: Acetyl group amount of modified EVOH resin (mole)

[0190] O: Hydroxyl amount of modified EVOH resin (mole)

[0191] C: The amount of aliphatic polyester grafted modified groups of modified EVOH resin (mole)

[0192] n: average chain length of aliphatic polyester units

[0193] E: Ethylene content of modified EVOH resin (mole)

[0194] X: aliphatic polyester graft modification ratio of modified EVOH resin (mol %).

[0195] [Manufacturing of modified EVOH resin composition]

[0196] As the titanium compound, titanium oxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used.

[0197] The titanium oxide was dry-blended with the obtained modified EVOH resin pellets so that the content of the titanium oxide in terms of metal became 0.1 ppm per unit mass of the EVOH resin composition to obtain a mixture.

[0198] The mixture was supplied to a twin-screw extruder (20 mm φ) equipped with a double-hole die, extruded under the following extrusion conditions, and the discharged strands were cooled and solidified in a water tank. Air was then blown into the solidified strands to remove water droplets on the strand surface, and then cut to obtain pellets of the modified EVOH resin composition.

[0199] [Extrusion conditions]

[0200] Extruder set temperature (℃): C1 / C2 / C3 / C4 / C5 / C6

[0201] =150 / 200 / 210 / 210 / 210 / 210

[0202] <Example 2>

[0203] In Example 1, pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that the blending amount of titanium oxide was changed to 1 ppm in terms of metal relative to the unit mass of the EVOH resin composition.

[0204] <Comparative Example 1>

[0205] Pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that titanium oxide was not used.

[0206] <Comparative Example 2>

[0207] In Example 1, pellets of a modified EVOH resin composition were obtained in the same manner as in Example 1 except that the blending amount of titanium oxide was changed to 10 ppm in terms of metal relative to the unit mass of the EVOH resin composition.

[0208] The following thermal stability evaluation was performed using the obtained pellets of the modified EVOH resin compositions of Examples 1 and 2 and Comparative Examples 1 and 2. The results are shown in Table 1 described below.

[0209] 〔Thermal stability evaluation〕

[0210] Using 5 mg of the obtained EVOH resin composition pellets, the weight was measured by a thermogravimetric measuring apparatus (manufactured by PerkinElmer, Pyris 1TGA) under nitrogen atmosphere, air flow rate: 20 mL / min, temperature: 230° C., time: 1 hour, and the weight reduction rate was calculated by the following formula. When this value is low, it means that the resin composition is not decomposed, which means that the thermal stability of the resin composition is excellent.

[0211] Weight reduction rate (%) = [(weight before heating - weight after heating) / weight before heating] × 100

[0212] [Table 1]

[0213]

[0214] According to Table 1, the EVOH resin compositions of Examples 1 and 2 containing a specific trace amount of titanium compound have a smaller weight reduction rate and excellent thermal stability than the EVOH resin composition of Comparative Example 1 not containing a titanium compound and the EVOH resin composition of Comparative Example 2 containing a titanium compound exceeding a specific range. In addition, a multilayer structure having a layer composed of the EVOH resin composition of Examples 1 and 2 can also obtain an effect of excellent thermal stability in which thermal degradation is suppressed.

[0215] The above embodiments show specific aspects of the present invention, but the above embodiments are merely illustrative and are not to be construed as limiting. It should be understood that various modifications obvious to those skilled in the art are within the scope of the present invention.

[0216] Industrial Applicability

[0217] Since the modified EVOH resin composition can suppress thermal degradation during melt molding, it is useful as a packaging material for various foods, as well as various packaging materials such as mayonnaise, salad dressing and other condiments, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, and pharmaceuticals.

Claims

1. A modified ethylene-vinyl alcohol copolymer composition, comprising a modified ethylene-vinyl alcohol copolymer containing an aliphatic polyester structural unit and a titanium compound, The metal equivalent content of the titanium compound is 0.001 ppm or more and less than 5 ppm based on the unit mass of the modified ethylene-vinyl alcohol-based copolymer composition. 2 . The modified ethylene-vinyl alcohol copolymer composition according to claim 1 , wherein the modification rate of the aliphatic polyester structural unit in the modified ethylene-vinyl alcohol copolymer is 0.1 to 30 mol %. 3 . The modified ethylene-vinyl alcohol copolymer composition according to claim 1 , wherein the average chain length of the aliphatic polyester structural units contained in the modified ethylene-vinyl alcohol copolymer is 1.5 to 3.

0. 4 . The modified ethylene-vinyl alcohol copolymer composition according to claim 1 , wherein the aliphatic polyester structural unit is a lactone ring-opening polymer. 5 . Pellets comprising the modified ethylene-vinyl alcohol copolymer composition according to claim 1 . 6 . A multilayer structure comprising at least one layer comprising the modified ethylene-vinyl alcohol copolymer composition according to claim 1 .

7. A method for producing a modified ethylene-vinyl alcohol copolymer composition, which is a method for producing the modified ethylene-vinyl alcohol copolymer composition according to any one of claims 1 to 4, The method comprises the step of melt-mixing a composition raw material containing the modified ethylene-vinyl alcohol-based copolymer and a titanium compound.

8. A method for producing a multilayer structure, which is a method for producing the multilayer structure according to claim 6, The method comprises the step of melt-molding a layer composed of the modified ethylene-vinyl alcohol copolymer composition.

Citation Information

Patent Citations

  • JP特开2019/163379

Cited By

  • Ethylene-vinyl alcohol copolymer resin composition as well as preparation method and application thereof

    CN119751727A

  • An ethylene-vinyl alcohol copolymer resin composition, a method for preparing the same, and an application thereof

    CN119751727B