Chitosan / polydopamine modified graphene oxide gel as well as preparation method and application thereof

By using chitosan/polydopamine modified graphene oxide gel in hair dyes, the health risks caused by strong oxidants in existing hair dyes and the poor stability of plant hair dyes are solved, and efficient and safe black hair dyeing is achieved. effect, and improves the adhesion durability and washability of hair dye.

CN118766796APending Publication Date: 2024-10-15SOUTH CHINA NORMAL UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410768323.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing hair dyes have scalp allergies and potential health risks caused by strong oxidants such as p-diphenylamine and its derivatives, and hydrogen peroxide. Plant hair dyes have poor stability, are easy to fade, and are complex to prepare. Bionic hair dyes have weak optical absorption properties in the visible light region. , poor adhesion durability, limiting its application.

Method used

Chitosan/polydopamine modified graphene oxide gel is used to graft dopamine onto graphene oxide and use dopamine to reduce graphene oxide to reduced graphene oxide to form a stable conjugated structure and enhance optical absorption. performance and adhesion durability, and uses chitosan as a dispersant and adhesive to improve adhesion firmness and durability.

Benefits of technology

A green and safe bionic hair dye is provided, which has a hair dyeing effect similar to that of a commercial oxidative hair dye, has good water washing resistance, maintains a short-term hair dyeing and color-fixing effect, and is suitable for semi-permanent hair dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004893295550000011
    Figure HDA0004893295550000011
  • Figure HDA0004893295550000021
    Figure HDA0004893295550000021
  • Figure HDA0004893295550000031
    Figure HDA0004893295550000031
Patent Text Reader

Abstract

The invention relates to the technical field of gel materials, and discloses chitosan / polydopamine modified graphene oxide gel as well as a preparation method and application thereof. The gel material is prepared from the following raw materials: dopamine, graphene oxide, chitosan, alkali liquor and ascorbic acid. The gel material provided by the invention is chitosan / polydopamine modified graphene oxide gel, and by grafting dopamine onto graphene oxide, the defects that a dopamine polymer is weak in optical absorption performance in a visible light region, poor in surface adhesion durability, poor in firmness and the like are effectively overcome; dopamine can be used as a green reducing agent to synchronously reduce graphene oxide into reduced graphene oxide, and the hydrophobicity of the reduced graphene oxide is beneficial to improving the waterproof performance of the gel; chitosan is used as a dispersing agent and an adhesive, helps to enhance the firmness and durability of gel adhesion, and can be applied to hair dyeing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gel materials, and in particular to a chitosan / polydopamine modified graphene oxide gel and a preparation method and application thereof. Background Art

[0002] Existing hair dyes can be divided into permanent and semi-permanent types. Permanent hair dyes include oxidative hair dyes and metallized dyes, and semi-permanent hair dyes include plant hair dyes and bionic hair dyes. Among them, oxidative hair dyes have the largest sales volume and have the characteristics of diverse hair dye colors and good color fastness. However, oxidative hair dyes contain strong oxidants such as p-diphenylamine and its derivatives, hydrogen peroxide, etc. People who use this type of hair dye for a long time are mostly troubled by symptoms such as scalp allergies and dermatitis. Metallized dyes have the potential risk of causing heavy metals to accumulate in the human body and causing leukemia. Plant hair dyes have the advantages of natural and safe color, good biocompatibility, wide source of raw materials and green safety, but have defects such as poor stability, easy fading, complex preparation process and high cost.

[0003] Bionic hair dyes are based on melanin and its analogs. At present, most black hair biomimetic hair dyes are developed based on the research and improvement of typical dopamine polymerization to produce human melanin, but related research still has the following shortcomings: (1) The weak optical absorption performance of dopamine and its polymers in the visible light region hinders their surface coloring and photothermal conversion, which is not conducive to their application in black dyes; (2) As the aging time of dopamine solution increases, the deposition rate of polydopamine coating on various substrates will decay rapidly, limiting its practical application; (3) The dyeing rate is low, the fastness is poor, and the preparation steps are cumbersome. These shortcomings seriously limit its commercial promotion and use. Summary of the invention

[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a gel material, which is a chitosan / polydopamine modified graphene oxide gel; the second purpose of the present invention is to provide a preparation method of the gel material; the third purpose of the present invention is to provide a hair dye; the fourth purpose of the present invention is to provide a gel material, or an application of a hair dye.

[0005] The basic principle of the present invention is described as follows:

[0006] Polydopamine (PDA) has similar structure and properties to human melanin, and is a typical melanin biomimetic with good polymerization and adsorption capabilities. Polydopamine can be formed by oxidative polymerization of its monomer dopamine (DA) under alkaline conditions. Graphene oxide (GO) is a two-dimensional carbon-based material composed of six-membered rings in a honeycomb lattice, with multiple active groups. Dopamine is grafted onto graphene oxide, and the graphene oxide is reduced to reduced graphene oxide (rGO) by utilizing the reducing property of dopamine. The resulting polydopamine reduced graphene oxide (PDA-rGO) has a stable conjugated structure, which can improve the optical absorption performance of the polymer in the visible light region and enhance the durability and firmness of the adhesion of the polydopamine solution on the hair surface.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] The first aspect of the present invention provides a gel material, comprising the following preparation raw materials: dopamine, graphene oxide, chitosan, alkali solution, and ascorbic acid.

[0009] Preferably, the mass ratio of dopamine to graphene oxide is 1:(0.4-3); further preferably, the mass ratio of dopamine to graphene oxide is 1:(1-1.5).

[0010] Preferably, the solid-liquid ratio of the graphene oxide to the alkali solution is 1 g: (80-300) mL; further preferably, the solid-liquid ratio of the graphene oxide to the alkali solution is 1 g: (130-150) mL.

[0011] Preferably, the pH of the alkali solution is 7.5-10.5.

[0012] Preferably, the alkaline solution comprises Tris-HCl buffer.

[0013] Preferably, the Tris-HCl buffer is prepared by a method comprising the following steps: dissolving tris (tris) in deionized water, fixing the volume, and adding hydrochloric acid solution dropwise to adjust the pH value to 7.5-10.5 to obtain the Tris-HCl buffer.

[0014] Preferably, the concentration of the trihydroxyaminomethane is 0.005-0.03 mol / L.

[0015] Preferably, the concentration of the hydrochloric acid is 0.05-0.3 mol / L.

[0016] Preferably, the solid-liquid ratio of the chitosan to the ascorbic acid solution is 1 g: (180-220) mL; further preferably, the solid-liquid ratio of the chitosan to the ascorbic acid solution is 1 g: (190-210) mL.

[0017] Preferably, the molecular weight of the chitosan is 190,000 to 310,000 Da.

[0018] Preferably, the concentration of the ascorbic acid solution is 1 to 5 mg / mL; more preferably, the concentration of the ascorbic acid solution is 1 to 3 mg / mL.

[0019] The second aspect of the present invention provides a method for preparing the gel material according to the first aspect of the present invention, comprising the following steps:

[0020] S1, dissolving chitosan in ascorbic acid solution, heating to obtain chitosan gel solution;

[0021] S2, mixing graphene oxide, dopamine and alkali solution, adjusting the pH, heating and polymerizing to obtain a polydopamine-reduced graphene oxide solution;

[0022] S3, mixing the chitosan gel solution with the polydopamine-reduced graphene oxide solution to obtain the gel material.

[0023] The present invention uses dopamine as a raw material to form polydopamine by oxidative polymerization under alkaline conditions, and grafts polydopamine onto graphene oxide under the action of a catalyst. Due to its excellent hydrophilicity, graphene oxide can react well with the amino group of polydopamine in a solution. During the process, dopamine can be used as a green reducing agent to simultaneously reduce graphene oxide to reduced graphene oxide, thereby forming polydopamine reduced graphene oxide (PDA-rGO). Polydopamine reduced graphene oxide can well form a smooth coating on the surface of a material, and at the same time, the transformation of graphene oxide from hydrophilicity to hydrophobicity can well play the role of waterproofing and protecting the coating. When applied to a bionic hair dye, the interaction between dopamine and hair can be enhanced.

[0024] Dissolving chitosan in ascorbic acid to form chitosan gel can improve the solubility and stability of chitosan in solution. Mixing chitosan gel with polydopamine-reduced graphene oxide to form chitosan / polydopamine-modified graphene oxide gel, chitosan gel plays the role of dispersant and adhesive, and can enhance the surface adhesion firmness and durability of polydopamine-reduced graphene oxide.

[0025] Preferably, in step S1, the heating temperature is 35-70°C; more preferably, the heating temperature is 55-65°C.

[0026] Preferably, in step S1, the heating time is 20 to 60 minutes; more preferably, the heating time is 30 to 50 minutes.

[0027] Preferably, in step S1, the heating method is water bath heating.

[0028] Preferably, in step S1, ultrasound is used as an aid.

[0029] Preferably, in step S2, graphene oxide is first mixed with alkaline solution under ultrasonic conditions for 20 to 40 minutes, and then mixed with dopamine.

[0030] Preferably, step S2 further comprises using a catalyst; the catalyst comprises 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC), and one of N-hydroxysuccinimide (NHS) and 4-dimethylaminopyridine (DMAP).

[0031] Preferably, the catalyst is used in an amount of 0.1 to 0.3 wt%.

[0032] Preferably, the mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide, or 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to 4-dimethylaminopyridine is 1:(0.8-1.2); further preferably, the mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to N-hydroxysuccinimide, or 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride to 4-dimethylaminopyridine is 1:(0.9-1.1).

[0033] Preferably, in step S2, the pH value is adjusted to 7.5-10.5.

[0034] Preferably, in step S2, an alkaline substance is added to adjust the pH; the alkaline substance includes at least one of sodium bicarbonate, sodium carbonate and ammonia water.

[0035] Preferably, in step S2, the temperature of the heating polymerization is 50-70°C; more preferably, the temperature of the heating polymerization is 55-65°C.

[0036] Preferably, in step S2, the heating polymerization time is 5 to 15 hours; more preferably, the heating polymerization time is 8 to 10 hours.

[0037] Preferably, in step S2, the heating polymerization is carried out by water bath heating.

[0038] Preferably, in step S3, the volume ratio of the polydopamine-reduced graphene oxide solution to the chitosan gel solution is 1:(0.2-2); further preferably, the volume ratio of the polydopamine-reduced graphene oxide solution to the chitosan gel solution is 1:(0.2-1).

[0039] The third aspect of the present invention provides a hair dye comprising the gel material according to the first aspect of the present invention.

[0040] The fourth aspect of the present invention provides use of the gel material described in the first aspect of the present invention, or the hair dye described in the third aspect of the present invention in hair dyeing.

[0041] Preferably, the hair dye is a bionic semi-permanent hair dye.

[0042] Preferably, the mass ratio of the gel material to the hair is 1:(1-2.5); further preferably, the mass ratio of the gel material to the hair is 1:(1-2).

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1) The gel material provided by the present invention is a chitosan / polydopamine modified graphene oxide gel. By grafting dopamine onto graphene oxide, the defects of dopamine polymer such as weak optical absorption performance in the visible light region, poor persistence of surface adhesion, and poor firmness are effectively solved; dopamine can be used as a green reducing agent to simultaneously reduce graphene oxide to reduced graphene oxide, and the hydrophobicity of reduced graphene oxide is beneficial to improving the waterproof performance of the gel; chitosan, as a dispersant and adhesive, helps to enhance the firmness and durability of gel adhesion.

[0045] 2) The preparation method of the gel material provided by the present invention has simple steps and is suitable for practical use.

[0046] 3) The hair dye provided by the present invention can dye white hair into black, which is green and safe, and the hair dyeing effect is similar to that of commercial oxidative hair dyes. It has good resistance to water washing after dyeing, can maintain a short-term hair dyeing and color fixing effect, and can be used as a semi-permanent hair dye. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The SEM images of graphene oxide (a), polydopamine-reduced graphene oxide (b) and the gel material of Example 1 (c);

[0048] Figure 2 SEM images of the surface (a) and cross-section (b) of natural white hair;

[0049] Figure 3 The SEM images of the surface (a) and cross section (b) of natural white hair after dyeing with the gel material of Example 1;

[0050] Figure 4 The figures are comparisons of natural white hair (a), hair samples dyed with the gel materials in Example 1 (b), Example 2 (c) and Example 3 (d), and hair samples dyed with the commercial hair dye (e) in Comparative Example 1;

[0051] Figure 5 The whiteness values ​​of natural white hair, white hair dyed with a commercial hair dye in Comparative Example 1, and white hair dyed with a gel material in Example 1;

[0052] Figure 6 This is a diagram showing the effect of the gel material in Example 1 being resistant to clean water washing;

[0053] Figure 7 This is a diagram showing the shampoo-resistant effect of the gel material in Example 1. DETAILED DESCRIPTION

[0054] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0055] Example 1

[0056] This embodiment provides a gel material, and the preparation method includes the following steps:

[0057] 1) Weigh 0.3029 g of tris(hydroxymethyl)aminomethane, put it into a 250 mL volumetric flask, add deionized water to make up to volume, prepare a 0.01 mol / L Tris solution, add 0.1 mol / L hydrochloric acid solution to adjust the solution to a pH of 8.5, and obtain a Tris-HCl buffer;

[0058] 2) Accurately weigh 150 mL of 2.5 mg / mL ascorbic acid solution into a 200 mL beaker, then accurately weigh 0.75 g of chitosan, dissolve the weighed chitosan in the ascorbic acid solution, and stir in a 60° C. water bath for 30 min to obtain a chitosan gel solution;

[0059] 3) Add 0.5 g of graphene oxide to 65 mL of Tris-HCl buffer, ultrasonicate for 30 min, stir evenly, then add 0.5 g of dopamine. Add catalysts EDC and DMAP (mass ratio 1:1, dosage 0.2 wt%), adjust the pH value to 8.5 with ammonia water, heat and stir in a 60 ° C water bath for 8 to 10 h to obtain a PDA-rGO solution, add 15 mL of chitosan gel to obtain a gel material.

[0060] Example 2

[0061] This embodiment provides a gel material, and the preparation method includes the following steps:

[0062] 1) Weigh 0.3029 g of tris(hydroxymethyl)aminomethane, put it into a 250 mL volumetric flask, add deionized water to make up to volume, prepare a 0.01 mol / L Tris solution, add 0.1 mol / L hydrochloric acid solution to adjust the solution to a pH of 8.5, and obtain a Tris-HCl buffer;

[0063] 2) Accurately weigh 150 mL of 2.5 mg / mL ascorbic acid solution into a 200 mL beaker, then accurately weigh 0.75 g of chitosan, dissolve the weighed chitosan in the ascorbic acid solution, and stir in a 60° C. water bath for 30 min to obtain a chitosan gel solution;

[0064] 3) Add 0.4 g of graphene oxide to 65 mL of Tris-HCl buffer, ultrasonicate for 30 min, stir evenly, then add 0.5 g of dopamine. Add catalysts EDC and DMAP (mass ratio 1:1, dosage 0.2 wt%), adjust the pH value to 8.5 with ammonia water, heat and stir in a 60°C water bath for 8 to 10 h to obtain a PDA-rGO solution, add 15 mL of chitosan gel to obtain a gel material.

[0065] Example 3

[0066] This embodiment provides a gel material, and the preparation method includes the following steps:

[0067] 1) Weigh 0.3029 g of tris(hydroxymethyl)aminomethane, put it into a 250 mL volumetric flask, add deionized water to make up to volume, prepare a 0.01 mol / L Tris solution, add 0.1 mol / L hydrochloric acid solution to adjust the solution to a pH of 8.5, and obtain a Tris-HCl buffer;

[0068] 2) Accurately weigh 150 mL of 2.5 mg / mL ascorbic acid solution into a 200 mL beaker, then accurately weigh 0.75 g of chitosan, dissolve the weighed chitosan in the ascorbic acid solution, and stir in a 60° C. water bath for 30 min to obtain a chitosan gel solution;

[0069] 3) Add 0.6 g of graphene oxide to 65 mL of Tris-HCl buffer, ultrasonicate for 30 min, stir evenly, then add 0.5 g of dopamine. Add catalysts EDC and DMAP (mass ratio 1:1, dosage 0.2 wt%), adjust the pH value to 8.5 with ammonia water, heat and stir in a 60°C water bath for 8 to 10 h to obtain a PDA-rGO solution, add 15 mL of chitosan gel to obtain a gel material.

[0070] Comparative Example 1

[0071] Taking commercial hair dye as a comparison, the commercial hair dye used is an oxidative black hair dye produced by Guangzhou Wenya Daily Cosmetics Co., Ltd. The main active ingredients of the hair dye are p-phenylenediamine, resorcinol, m-aminophenol, ethanolamine, sodium sulfite, ammonium hydroxide, sodium isoascorbate, and hydrogen peroxide.

[0072] Performance Testing

[0073] 1) observing the morphology of graphene oxide, polydopamine-reduced graphene oxide, and the gel material of Example 1 using a scanning electron microscope;

[0074] 2) Observe the surface and cross-section morphology of natural white hair using a scanning electron microscope;

[0075] 3) using a scanning electron microscope to observe the morphology of the surface and cross section of natural white hair after dyeing with the gel material of Example 1, wherein the amount of the gel material of Example 1 used is 10 g / 15 g of hair;

[0076] 4) The whiteness of natural white hair, white hair dyed with the gel material of Example 1, and white hair dyed with the commercial hair dye of Comparative Example 1 was measured using an automatic whiteness meter (WSD-3C), wherein the amount of the gel material of Example 1 and the commercial hair dye of Comparative Example 1 was 10 g / 15 g of hair; generally, a whiteness value less than 30 is considered to be blackening of the hair, and the lower the whiteness value, the darker the hair color:

[0077] The hair samples to be measured were laid flat on the measuring board. The whiteness values ​​of natural white hair and black hair dyed with the commercial hair dye in Comparative Example 1 were measured first as reference values, and the hair samples dyed with the gel material in Example 1 were measured last. To reduce the random error of the experiment, each measurement object was measured 5 times, and the L, a, and b values ​​of each measurement were obtained by whiteness meter and the average value was taken. The average value of these three values ​​was calculated using Hunterlab color measurement system, and the whiteness value calculation equation was: Among them, Wh is the whiteness value, L is the lightness value, a and b are the chromaticity values, and each data and dyeing situation is recorded.

[0078] 5) Washing resistance test:

[0079] Perform the elution experiment with clean water and shampoo at the same time. Place the sample hair dyed with the gel material of Example 1 into a centrifuge tube, and add clean water and water containing 5% shampoo respectively. Then place it in an oscillator and adjust the speed to simulate the shampooing scene. After the end, place the sample hair in a ventilated place to dry naturally and observe the coloring. Repeat the above operation, counting each 5-minute wash as 1 time, wash 5 times, 10 times, 20 times and 30 times respectively, and observe the color change of the sample hair during the whole process.

[0080] Figure 1The SEM images of graphene oxide (a), polydopamine-reduced graphene oxide (b) and the gel material of Example 1 (c) are shown in FIG. Figure 1 (a) It can be seen that the graphene oxide has a sheet structure. In some areas, the graphene oxide sheets are multi-layered and overlapped, while in some areas, they are distributed in a single layer. This is because oxidation causes the graphene layer to generate epoxy groups, hydroxyl groups, etc., which intensifies the repulsion between the layers and facilitates the peeling of the graphene layer. Figure 1 (b) It can be seen that the repulsion between layers in polydopamine-reduced graphene oxide is reduced, and there are layers with low overlap. The overlap of layers causes the rugged wrinkles on the surface; Figure 1 (c) It can be seen that after adding chitosan, chitosan covers the surface of polydopamine-reduced graphene oxide to form a complex structure. Many protrusions can be seen on the surface. These structures are conducive to the formation of a coating on the hair surface by the hair dye gel.

[0081] Figure 2 SEM images of the surface (a) and cross-section (b) of natural white hair. Figure 2 (a) It can be seen that in the scale layer on the surface of natural white hair, the scales are densely and orderly distributed with a certain regularity and the surface is smooth overall; Figure 2 (b) It can be seen that the cross-section of natural white hair has clean and smooth edges.

[0082] Figure 3 The surface (a) and cross-section (b) SEM images of natural white hair after dyeing with the gel material of Example 1. Figure 3 (a) It can be seen that after dyeing, the hair scales on the surface of white hair disappear and the surface has a uniform coating; Figure 3 (b) It can be seen that the edge of the white hair is covered by a layered material, and there are scattered raised flake-like substances on the edge of the cross section, which are gel materials covering the surface of the hair, indicating that the hair dye gel has adhered well to the surface of the hair.

[0083] Figure 4 The figures are comparison diagrams of natural white hair (a), hair dyed with the gel materials in Example 1 (b), Example 2 (c) and Example 3 (d), and hair dyed with the commercial hair dye in Comparative Example 1 (e); Figure 4 It can be seen from (b) to (d) that after dyeing with the gel material in Examples 1 to 3, the hair sample has a dark color, which is similar to the color of black hair (e) dyed with a commercial hair dye, indicating that the gel material in Examples 1 to 3 has a similar hair dyeing effect as the commercial oxidative black hair dye.

[0084] Figure 5 The whiteness values ​​of natural white hair, white hair dyed with commercial hair dye in comparative example 1, and white hair dyed with gel material in example 1 are given by Figure 5It can be seen that after dyeing with the gel material of Example 1, the whiteness value of the white hair is greatly reduced, and is even lower than the whiteness value of the hair dyed with a commercial oxidative black hair dye.

[0085] Figure 6 This is a diagram showing the effect of the gel material in Example 1 on water washing resistance. From left to right, they are natural white hair, hair sample without washing after dyeing, hair sample washed 5 times after dyeing, hair sample washed 10 times after dyeing, hair sample washed 20 times after dyeing, and hair sample washed 30 times after dyeing. Figure 6 It can be seen that after washing with clean water 5 times, the color of the hair sample becomes slightly lighter. During the washing process of 5 to 30 times, the color of the hair sample does not change much, indicating that the gel material of Example 1 has a certain waterproof ability. After the gel forms a coating on the surface of the hair sample, the dyed hair sample has better water washing resistance and less color fading.

[0086] Figure 7 The shampoo-resistant effect of the gel material in Example 1 is shown in Figure 1. From left to right, they are natural white hair, unwashed hair after dyeing, hair washed 5 times after dyeing, hair washed 10 times after dyeing, hair washed 20 times after dyeing, and hair washed 30 times after dyeing. Figure 7 It can be seen that when the hair is washed with shampoo for 5 to 10 times, the color of the hair becomes slightly lighter. When the hair is washed for 20 to 30 times, the black color becomes lighter faster and the color fading becomes more severe, indicating that the gel material of Example 1 can maintain a short-term hair dyeing and fixing effect and can be used as a semi-permanent hair dye.

[0087] In the gel material provided by the present invention, polydopamine is a typical melanin biomimetic, which has the advantages of being green and safe, and overcomes the defects of scalp allergies and dermatitis easily caused by substances such as p-diphenylamine and its derivatives, hydrogen peroxide and other strong oxidants in oxidative hair dyes; the gel material has adhesion stability on the hair surface, has a hair dyeing effect similar to that of commercial oxidative black hair dyes, has excellent water-washing resistance, and has a good short-term hair dyeing and color fixing effect, and can be used as a semi-permanent hair dye.

Claims

1. A gel material, characterized in that: The preparation method comprises the following raw materials: dopamine, graphene oxide, chitosan, alkali solution and ascorbic acid.

2. The gel material according to claim 1, characterized in that: The mass ratio of dopamine to graphene oxide is 1: (0.4~3); And / or, the solid-liquid ratio of the graphene oxide to the alkali solution is 1 g: (80-300) mL; and / or, the pH value of the alkali solution is 7.5 to 10.5; And / or, the alkaline solution comprises Tris-HCl buffer.

3. The gel material according to claim 1, characterized in that: The solid-liquid ratio of the chitosan to ascorbic acid solution is 1 g: (180-220) mL; And / or, the molecular weight of the chitosan is 190000-310000Da; And / or, the concentration of the ascorbic acid solution is 1-5 mg / mL.

4. The method for preparing the gel material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, dissolving chitosan in ascorbic acid solution, heating to obtain chitosan gel solution; S2, mixing graphene oxide, dopamine and alkali solution, adjusting the pH, heating and polymerizing to obtain a polydopamine-reduced graphene oxide solution; S3, mixing the chitosan gel solution with the polydopamine-reduced graphene oxide solution to obtain the gel material.

5. The preparation method according to claim 4, characterized in that: In step S1, the heating temperature is 35-70°C; And / or, the heating time is 20 to 60 minutes.

6. The preparation method according to claim 4, characterized in that: The step S2 further includes using a catalyst; the catalyst includes 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and one of N-hydroxysuccinimide and 4-dimethylaminopyridine.

7. The preparation method according to claim 4, characterized in that: In the step S2, the temperature of the heating polymerization is 50-70°C; And / or, the heating polymerization time is 5 to 15 hours.

8. The preparation method according to claim 4, characterized in that: In the step S3, the volume ratio of the polydopamine-reduced graphene oxide solution to the chitosan gel solution is 1:(0.2-2).

9. A hair dye, characterized in that: The invention comprises the gel material according to any one of claims 1 to 3.

10. Use of the gel material according to any one of claims 1 to 3, or the hair dye according to claim 9 in hair dyeing.

Citation Information

Cited By

  • Plant essential oil mosquito-repellent slow-release gel and preparation method thereof

    CN119404864A

  • Lightweight warm-keeping comfortable garment material and preparation method thereof

    CN119531150A