Piezoelectric composite hydrogel for promoting bone repair and preparation method thereof
By preparing a piezoelectric composite hydrogel combining nano-Ag-BaTiO3 and carboxymethyl chitosan, and utilizing its piezoelectricity and biocompatibility, the problems of drug side effects and surgical trauma in the treatment of bone injuries have been solved, and bone damage has been achieved. Effective regeneration and repair of tissue.
Patent Information
- Application Number
- CN202411032021.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-15
AI Technical Summary
Existing bone injury treatment methods have problems such as drug side effects, large surgical trauma, and high risk of infection. Commonly used bone repair materials are difficult to apply to irregular bone defects, and long-term use may lead to mechanical failure.
Nano-BaTiO3 is mixed with silver ammonia solution to prepare nano-Ag-BaTiO3, combined with carboxymethyl chitosan and growth factors, and a piezoelectric composite hydrogel is prepared through cross-linking reaction. Its piezoelectricity and biocompatibility are used to promote bone cells. Penetration and migration, establishing an electric field to stimulate bone tissue regeneration.
While ensuring the overall performance of the material, it promotes the production of bone extracellular matrix, enhances bone tissue regeneration, reduces the risk of infection, avoids mechanical failure, and achieves effective repair of bone tissue.
Smart Images

Figure CN118767216A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric hydrogels, and in particular to a piezoelectric composite hydrogel for promoting bone repair and a preparation method thereof. Background Art
[0002] Human or animal bone tissue has a certain ability to regenerate and remodel after mechanical stimulation and injury. However, with age, the repair ability of bone tissue itself will decline significantly, and may cause corresponding complications. Bone regeneration and repair involves the coordinated regulation of multiple biological processes, which jointly guide homeostasis and tissue regeneration in the body. In the bone tissue microenvironment, growth factors, mechanical stimulation, and the interaction of the extracellular matrix (ECM) are all key factors affecting bone regeneration. Due to the regulation of cells and growth factors, the supply of growth factors in bone and cartilage defect areas is limited, and it is necessary to rely on alternative materials to deliver growth factors to assist in bone defect repair.
[0003] At present, the treatment of bone injuries is still mainly aimed at alleviating related pathological symptoms, while the main goal is to repair the bone defect.
[0004] Generally speaking, the treatment of bone injuries is mainly divided into drug treatment and surgical treatment.
[0005] (1) Drug treatment: When bone damage is not serious, drug treatment can be used first, and other methods, such as changing lifestyle and proper exercise, can effectively alleviate bone damage. However, the disadvantage of drug treatment is that it is mainly used for bone damage with mild symptoms, and the drugs have related side effects.
[0006] (2) Surgical treatment: Surgical treatment is a mainstream method for treating bone injuries, which mainly includes: bone marrow stimulation, mosaic formation surgery, bone cell implantation, etc. It can effectively repair damaged bone tissue, but the trauma caused by surgical treatment is far greater than the side effects of drug treatment, and there are risks of infection with infectious diseases, immune rejection, etc.
[0007] Among them, the materials commonly used for bone repair mainly include medical metals, bioceramics, biopolymers and their related composite materials. However, most medical metal materials and bioceramics require secondary surgery to remove after tissue healing, which not only increases medical costs but also increases the morbidity of patients. In addition, although such bone repair materials have shown good osteoinductivity and osteoconductivity, due to their inherent properties, their application in irregular bone defect sites is difficult, and long-term presence in the body may cause mechanical failure of the implant site. Summary of the invention
[0008] In order to solve the above technical problems, a technical solution adopted by the present invention is: Provided is a piezoelectric composite hydrogel for promoting bone repair and a preparation method thereof, the steps comprising: (1) mixing nano BaTiO3 powder with silver ammonia solution to obtain nano Ag-BaTiO3; (2) Using carboxymethyl chitosan as a dispersant, nano-Ag-BaTiO3 and transforming growth factor are mixed and added to the gel precursor, and then a curing agent is added to cause a cross-linking reaction to obtain a piezoelectric composite hydrogel.
[0009] In a preferred embodiment of the present invention, the mass ratio of the nano-BaTiO3 powder to the silver ammonia solution is:.
[0010] In a preferred embodiment of the present invention, the mass ratio of the carboxymethyl chitosan, the nano-Ag-BaTiO3 and the transforming growth factor is:.
[0011] In a preferred embodiment of the present invention, the growth factor includes one or more of bone morphogenetic protein BMP, bone-derived growth factor BDGF, and growth transfer factor TGF-β1.
[0012] In a preferred embodiment of the present invention, the gel precursor is methacrylated gelatin, or a combination of one or more thereof.
[0013] In a preferred embodiment of the present invention, the carboxymethyl chitosan is obtained by subjecting chitosan to carboxymethylation reaction in alkaline solution.
[0014] In a preferred embodiment of the present invention, the curing agent is an ultraviolet curing agent.
[0015] In a preferred embodiment of the present invention, the methacrylated gelatin is prepared by first swelling gelatin, then mixing with methacrylic anhydride and then dialyzing.
[0016] A piezoelectric composite hydrogel for promoting bone repair, comprising a piezoelectric composite hydrogel prepared by the preparation method described in any one of claims 1 to 8.
[0017] A piezoelectric composite hydrogel patch for promoting bone repair, comprising a piezoelectric composite hydrogel layer prepared by the preparation method described in any one of claims 1 to 8, and a backing layer and a PC isolation layer respectively arranged on both sides of the piezoelectric composite hydrogel layer.
[0018] The beneficial effects of the present invention are: growth factors are added to the GelMA hydrogel to induce the formation of new bone tissue by promoting the generation of extracellular matrix of bone cells, and piezoelectric Ag-BaTiO3 and positively charged carboxymethyl chitosan are added to effectively promote cell penetration and migration, and promote the regeneration of bone tissue together with growth factors, thereby preparing Ag-BaTiO3 / CMCS / growth factor / piezoelectric composite hydrogel, while ensuring the overall performance of the composite hydrogel material, using the piezoelectric properties of bone tissue and the self-powered characteristics of piezoelectric materials to establish an electric field in situ, thereby achieving the purpose of stimulating bone tissue regeneration. . BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which: Figure 1 is a flow chart of the preparation of the GelMA hydrogel matrix of Example 1 of the present invention; Figure 2 This is a schematic diagram of the structure of the ultrasound body and the piezoelectric composite hydrogel in Example 1 of the present invention; Figure 3 is a TEM image of Ag-BaTiO3 of Example 1 of the present invention; Figure 4 is the EDS spectrum of Ag-BaTiO3 of Example 1 of the present invention; Figure 5 is the XRD spectrum of Ag-BaTiO3 in Example 1 of the present invention; Figure 6 is a SEM image of the piezoelectric composite hydrogel of Example 1 of the present invention; Figure 7 is a phase change diagram of the piezoelectric composite hydrogel in Example 1 of the present invention; Figure 8 This is a test diagram of the adhesion performance of the piezoelectric composite hydrogel in Example 1 of the present invention; Fig. 9 is a result diagram of the swelling rate of the piezoelectric composite hydrogel in Example 1 of the present invention; Fig.10 is a graph showing the porosity of the piezoelectric composite hydrogel of Example 1 of the present invention; Fig.11 is a diagram showing the cytotoxicity test results of the piezoelectric composite hydrogel in Example 1 of the present invention; Fig.12 This is a graph showing the antibacterial rate experimental results of the piezoelectric composite hydrogel in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] See also Figure 1-12 , the embodiment of the present invention includes: A piezoelectric composite hydrogel for promoting bone repair, the raw materials of which include: a GelMA hydrogel matrix and nano-BaTiO3 particles, silver nano-particles, carboxymethyl chitosan and growth factors loaded in the GelMA hydrogel matrix.
[0022] Nano-BaTiO3 particles have excellent piezoelectric properties and good biocompatibility. After introducing silver nanoparticles into nano-BaTiO3, due to the good conductivity of silver nanoparticles, during the polarization process, silver nanoparticles can form numerous microcapacitors to enhance the effective dielectric constant of nano-BaTiO3, thereby enhancing the polarization electric field of nano-BaTiO3. Strong electric fields can cause the electric domains of nano-BaTiO3 to be arranged along the direction of the electric field, so that the piezoelectricity of nano-BaTiO3 can be better exerted, thereby further improving the piezoelectricity of hydrogels. At the same time, silver nanoparticles are also a common broad-spectrum antibacterial agent with good biocompatibility and strong bactericidal ability. They can effectively improve antibacterial properties, so as to keep the microenvironment of the bone repair site sterile, avoid wound infection, and facilitate bone repair.
[0023] Among them, piezoelectric materials are a typical force-electric conversion material that can convert various mechanical stimuli into electrical signals or convert alternating electrical signals into mechanical vibrations based on the piezoelectric effect. It is one of the best choices for generating local electrical stimulation signals that cause changes in internal potential caused by deformation under external force. Because bones themselves have piezoelectric characteristics, piezoelectric materials with electrical responses can be used to simulate and amplify continuous piezoelectric currents to promote endogenous "bioelectricity" for bone repair and regeneration, which can promote bone healing and is a preferred bone repair material.
[0024] Carboxymethyl chitosan has osteoconductivity, which enables it to play an important role in bone repair. In addition, carboxymethyl chitosan can promote the infiltration and migration of macrophages and neutrophils, remove foreign matter, and further promote wound repair.
[0025] Growth factors can not only promote the proliferation, differentiation and maturation of bone cells, but also stimulate cells to produce sufficient extracellular matrix, promote and accelerate the formation of bone and cartilage tissue. Growth factors include bone morphogenetic protein (BMP), bone-derived growth factor (BDGF), growth transfer factor (TGF-β1), etc. Among them, bone morphogenetic protein (BMP): has a long-term induction of bone formation and can accelerate the formation of new bones; bone-derived growth factor (BDGF): can stimulate bone cell proliferation and collagen, promote cartilage formation, and increase the number of chondrocytes; growth transfer factor (TGF-β): contains rich bone components and can promote bone cell growth.
[0026] Since the use of growth factors usually needs to be combined with biological carrier materials for local delivery in order to control the release dose and release kinetics of the growth factors, thereby increasing the retention time of the growth factors at therapeutic concentrations, this application uses GelMA hydrogel as a delivery carrier because GelMA hydrogel is a new type of highly hydrated polymer material with good biocompatibility and low immune response, and is currently an ideal biological carrier material.
[0027] The GelMA hydrogel matrix was selected as the loading system for various drugs, and functional BaTiO3 particles, silver nanoparticles and growth factors were introduced into the polymer network structure to construct a piezoelectric composite hydrogel material. Since the nanoparticles have a high specific surface area, they can form a tight binding interface with the polymer matrix, thereby achieving the regulation of the mechanical and biological properties of the hydrogel, so that each component can fully exert its efficacy, effectively making up for the shortcomings of a single component in bone repair performance. At the same time, it can also effectively control the release rate and regulate the internal cross-linking network of the hydrogel and mediate protein adsorption, cell differentiation and tissue regeneration, thereby continuously producing a therapeutic and repair effect on bone tissue.
[0028] like Figure 2 As shown, the structure of a piezoelectric composite hydrogel patch for promoting bone repair includes: a hydrogel layer 1 made of piezoelectric composite hydrogel, a backing adhesive layer 2 arranged on the back of the hydrogel layer, and an isolation layer 3 arranged on the front of the hydrogel layer to keep the moisture of the hydrogel. In actual use, the isolation layer is torn off to contact the piezoelectric composite hydrogel with the human body, and then the ultrasonic transmitter body 4 is attached (adhesive) to the backing tape to apply ultrasonic waves in vitro, thereby utilizing the drug sustained release characteristics of the hydrogel to achieve the regulation of the drug sustained release rate.
[0029] Among them, the excitation transducer that generates the excitation electrical signal is composed of a transmitting circuit. The frequency of the excitation signal is determined by the center frequency of the transducer, covering a range of 20KHz-2 MHz, and the excitation voltage is in the range of 0-20 V. The excitation waveform can be a pulse wave, a square wave, a sine wave, etc. The excitation electrical signal can be one or more continuous pulses, and its duty cycle can be adjusted as needed. The excitation signal can be a pulse excitation or a continuous wave excitation.
[0030] In addition, considering the actual needs of portability or wearability, the ultrasonic equipment required here should be simple and portable and have a small body size. The diameter of the generally used ultrasonic body is 3-5 cm, which can be easily applied in the actual scenario of bone repair.
[0031] By combining piezoelectric composite hydrogel materials with ultrasound, not only can the release rate of growth factors be regulated by controlling the time and intensity of electrical stimulation in the body, but also, due to the low attenuation of energy transmitted to bone tissue and the deep penetration distance, low-intensity pulsed ultrasound can directly act on bone tissue, subcutaneous tissue and nerve tissue, etc., and can also cause calcium salt deposition in bone tissue. That is, low-intensity pulsed ultrasound can enhance the therapeutic effect of piezoelectric composite hydrogel and promote bone tissue healing.
[0032] The contents of the raw materials of the piezoelectric composite hydrogel are as follows: Provided is a method for preparing a piezoelectric composite hydrogel for promoting bone repair, comprising the synthesis of nano-BaTiO3, the synthesis of Ag-BaTiO3, the synthesis of a methacrylated hydrogel matrix, and the preparation of an Ag-BaTiO3 / CMCS / growth factor / GelMA piezoelectric hydrogel; using carboxymethyl chitosan as a dispersant, then mixing Ag-BaTiO3 and growth factor into a gel precursor, then placing the mixture in a 30-40°C water bath for rapid dissolution and mixing, then adding an ultraviolet curing agent (LAP), and irradiating with an ultraviolet lamp for a photo-crosslinking reaction, thereby obtaining a piezoelectric composite hydrogel, wherein the specific steps include: (1) Synthesis of nano BaTiO3 powder: (1.1) Prepare 5-20 mol / L NaOH aqueous solution, use a measuring cylinder to measure 40-80 mL of NaOH aqueous solution, add 0.5-1.5 g of TiO2, and stir until uniform; (1.2) Transfer the above solution to a polytetrafluoroethylene liner and seal it in a stainless steel autoclave, transfer the autoclave to an oven, and heat the reaction at 120-240°C for 12-36 hours; (1.3) After the reaction is completed, the solid product is repeatedly rinsed with deionized water and anhydrous ethanol for several times, and then placed in 20-100 mL of a 5-8% dilute hydrochloric acid aqueous solution and stirred for reaction for 5-10 hours; (1.4) After stirring, rinse with deionized water and anhydrous ethanol several times, put the product into an oven and dry it at a constant temperature of 50-70℃ for 6-12 hours; (1.5) Prepare a 0.05-0.2 mol / L Ba(OH)2·8H2O aqueous solution, add the above product to the Ba(OH)2·8H2O aqueous solution and stir evenly, transfer the mixed solution to a polytetrafluoroethylene liner, and seal it in a stainless steel autoclave, transfer the autoclave to an oven, and heat the reaction at 140-240°C for 12-48 hours; (1.6) After the reaction is completed, the solid product is repeatedly rinsed with deionized water and anhydrous ethanol for several times, and the product is placed in an oven and dried at a constant temperature of 50-70°C for 6-12 hours; (1.7) Grind the dried product in a mortar for 10-30 minutes to obtain nano-BaTiO3 powder material.
[0033] (2) Synthesis of Ag-BaTiO3: (2.1) Add 28% ammonia water to 0.5 mol / L silver nitrate solution at a volume ratio of 1:10 to prepare a silver ammonia solution, then add 0.1-1 g of nano BaTiO3 powder to the silver ammonia solution and stir to react for 2-8 hours; (2.1) Pour the above suspension into a centrifuge tube, collect the solid product with a high-speed centrifuge, and then repeatedly rinse it with deionized water. Put the product into an oven and dry it at a constant temperature of 50-70°C for 6-12 hours. Finally, grind the dried product with a mortar for 10-30 minutes to obtain nano-Ag-BaTiO3 material.
[0034] (3) Synthesis of carboxymethyl chitosan (CMCS): (3.1) Weigh 0.5-2 g of chitosan, mix with an organic solvent such as ethanol or isopropanol, stir evenly, and soak for 4 hours; (3.2) Add the above solution to a 30%-50% sodium hydroxide solution for alkalization reaction for 2-4 hours, then add chloroacetic acid to the alkalized carboxymethyl chitosan solution for carboxymethylation reaction, control the temperature at 45-55°C, react for 4 hours, and then terminate the reaction; (3.3) The reaction product is repeatedly washed and filtered with ethanol for 3-5 times, then placed in a vacuum drying oven for drying, and finally ground with a mortar to produce carboxymethyl chitosan.
[0035] (4) Synthesis of methacrylated gelatin (GelMA): (4.1) Dissolve an appropriate amount of gelatin in 200 mL of 30-40℃ deionized water and allow to swell at room temperature for several hours; (4.2) Stir and dissolve at 50-60℃ for several hours, then slowly drop 6-9 mL of methacrylic anhydride, react at 50-60℃ for several hours with continuous stirring; (4.3) Add 200 mL of 30-40℃ deionized water to dilute and terminate the reaction; (4.4) Place the above solution into a dialysis bag and place the dialysis bag in deionized water at 30-50 °C for 5-7 days to remove unreacted monomers. Change the water every 2-4 hours. (4.5) The dialyzed solution was transferred to a petri dish to cool, and the obtained material was collected by vacuum freeze drying.
[0036] (5) Preparation of Ag-BaTiO3 / CMCS / growth factor / GelMA piezoelectric composite hydrogel: (5.1) Weigh 0.1 g-0.5 g of GelMA and dissolve it in 1-2 mL of deionized water to prepare a GelMA solution; (5.2) Weigh 20-100 mg of Ag-BaTiO3 and 50 mg of CMCS, add them to the GelMA solution and stir slowly for 1-3 hours; (5.3) Add 5-25 mg of growth factor and quickly stir the mixture evenly; (5.4) Add 0.1-0.5g of light curing agent (LAP), heat to 40-50℃ and stir for 5-10 minutes in a completely dark environment; (5.5) Use a disposable sterile medical needle to draw up the mixed solution and add it into a suitable mold; (5.6) Under completely light-proof conditions, a photo-crosslinking reaction is carried out under ultraviolet light to obtain a piezoelectric composite hydrogel. Example
[0037] A method for preparing a piezoelectric composite hydrogel for promoting bone repair comprises the following steps: (1) Synthesis of nano-BaTiO3 powder: Add 0.5 g of TiO2 to 40 mL of 5 mol / L NaOH aqueous solution and stir until uniform; seal the solution in a stainless steel autoclave and heat at 120 °C for 12 hours; after the reaction, rinse the solid product with deionized water and anhydrous ethanol several times, then put it into 20 mL of 5% dilute hydrochloric acid aqueous solution and stir for 5 hours; after stirring, rinse it with deionized water and anhydrous ethanol several times, put the product in an oven and dry it at 50 °C for 6 hours; add the dried product to 0.05 mol / L Ba(OH)2·8H2O aqueous solution and stir until uniform, then seal the mixed solution in a stainless steel autoclave and heat at 140 °C for 12 hours. hours; after the reaction is completed, the obtained solid product is repeatedly washed with deionized water and anhydrous ethanol for several times, and the product is placed in an oven and dried at a constant temperature of 50°C for 6 hours; the dried product is ground in a mortar for 10 minutes to obtain a nano-BaTiO3 powder material.
[0038] (2) Synthesis of Ag-BaTiO3: 2 mL of ammonia water was added dropwise to 0.2 mL of 0.5 mol / L silver nitrate solution to prepare a silver-ammonia solution. Subsequently, 0.1 g of nano-BaTiO3 powder was added to the silver-ammonia solution and stirred for 2 hours. The above suspension was poured into a centrifuge tube, and the solid product was collected by a high-speed centrifuge. The solid product was then repeatedly rinsed with deionized water and placed in an oven for constant temperature drying at 50°C for 6 hours. Finally, the dried product was ground in a mortar for 10 minutes to obtain nano-Ag-BaTiO3 material.
[0039] (3) Synthesis of carboxymethyl chitosan (CMCS): Weigh 0.5 g of chitosan, add 50 mL of ethanol or isopropanol as an organic solvent, stir until uniform, and soak for 4 hours; add the above solution to a 30% sodium hydroxide aqueous solution, alkalize for 1 hour, then add chloroacetic acid to the alkalized chitosan solution for carboxymethylation, control the reaction temperature at 60 °C, react for 4 hours, and wait to cool to room temperature; wash the reaction product repeatedly with ethanol and filter it three times, then put it into a vacuum drying oven for drying, and finally grind it in a mortar to make carboxymethyl chitosan.
[0040] (4) Synthesis of methacrylated gelatin (GelMA): Dissolve 5 g of gelatin in 200 mL of 40°C deionized water and swell at room temperature for several hours; stir and dissolve at 60°C for several hours, then slowly drop 6 mL of methacrylic anhydride and react at 60°C for several hours with continuous stirring; add 200 mL of 40°C deionized water to dilute and terminate the reaction; place the above solution in a dialysis bag and dialyze the dialysis bag in 45°C deionized water for 7 days to remove unreacted monomers, changing the water every 4 hours; transfer the dialyzed solution to a culture dish to cool, and collect the material by vacuum freeze drying.
[0041] (5) Preparation of Ag-BaTiO3 / CMCS / growth factor / GelMA piezoelectric composite hydrogel: Weigh 0.1 g of GelMA and dissolve it in 1 mL of deionized water to prepare a GelMA solution; weigh 20 mg of Ag-BaTiO3 and 50 mg of CMCS and add them to the GelMA solution and stir slowly for 3 h; add 5 mg of growth factor and quickly stir the mixture to make it uniform; add 0.1 g of photocuring agent (LAP) and heat to 50 °C and stir for 5-10 min in a completely dark environment; use a disposable sterile medical syringe to draw up the uniformly stirred mixture and add it to a suitable mold; irradiate with ultraviolet light in a completely dark environment to carry out a photocrosslinking reaction to obtain a piezoelectric composite hydrogel.
[0042] Comparative Example 1, Comparative Example 2 and Comparative Example 3 are configured for comparative testing, wherein: The main components of Comparative Example 1 are the same as those of Example 1, except that the raw material ingredients do not contain growth factors; The main components of Comparative Example 2 are the same as those of Example 1, except that the raw material composition does not contain Ag-BaTiO3; The main components of Comparative Example 3 are the same as those of Example 1, except that the raw material ingredients do not contain carboxymethyl chitosan.
[0043] Performance Test: The morphology and structure of the piezoelectric composite hydrogel samples were characterized by TEM, EDS, SEM, XRD, XPS, Raman, FT-IR, NMR, etc.: 1. As Figure 3 As shown, it can be seen from the TEM image that the size of Ag-BaTiO3 nanoparticles is uniform, and the silver nanoparticles are evenly embedded on the surface of the barium titanate nanoparticles; 2. If Figure 4 and Figure 5 As shown, it can be seen from the EDS and XRD spectra that Ag-BaTiO3 was successfully prepared; 3. Such as Figure 6 As shown, it can be seen from the SEM microscopic morphology that the piezoelectric composite hydrogel is a porous material with a pore size of approximately 100-200 microns.
[0044] The physical and chemical properties of the piezoelectric composite hydrogel were tested, including phase change, adhesion test, swelling rate test, and porosity test.
[0045] Phase change: like Figure 7 The diagram shows the phase change of the piezoelectric composite hydrogel prepared in Example 1. As can be seen from the picture, after UV cross-linking, the sol in the mold turns into a gel state, and the gel loaded with Ag-BaTiO3 is beige.
[0046] Adhesion performance test: like Figure 8 The figure shows the adhesion performance test of the piezoelectric composite hydrogel prepared in Example 1. It can be seen that the hydrogel has good adhesion and does not leave any residue after being removed from the skin surface.
[0047] Swelling rate test: The piezoelectric composite hydrogel was freeze-dried, and each sample was about 100-200 mg (denoted as W1), and immersed in a beaker containing 100-200 mL of phosphate buffer solution at room temperature. The sample was taken out at a certain time interval, and the water on the surface of the hydrogel was absorbed by filter paper and weighed. The weight was expressed as W2. According to the formula Calculate the swelling ratio, such as Fig. 9 As shown in the figure. The swelling ratios of GelMA and Ag-BaTiO3 / CMCS / growth factor / GelMA are 492% and 537%, respectively. It can be found that the swelling performance of the piezoelectric composite hydrogel is slightly higher than that of GelMA. This is because carboxymethyl chitosan can reduce the pore size of the gel, increase the specific surface area, increase the water swelling behavior, and reduce the flexibility, thereby increasing the swelling ratio of the gel.
[0048] Porosity test: Weigh a quantitative volume of ethanol (recorded as V1), then soak the sample in ethanol, and the total volume of the sample and ethanol is recorded as V2. After soaking for several hours, take out the sample and record the volume at this time (recorded as V3), and then calculate the volume according to the formula Calculate the porosity, such as Fig.10 As shown in Figure 2, the porosity of GelMA and Ag-BaTiO3 / CMCS / growth factor / GelMA are 72.6% and 68.9%, respectively. It can be seen that compared with GelMA hydrogel, the porosity of the hydrogel decreases after adding Ag-BaTiO3 and carboxymethyl chitosan.
[0049] The piezoelectric composite hydrogel is subjected to biological performance tests, including biocompatibility tests and antibacterial performance tests.
[0050] Biocompatibility test: The piezoelectric composite hydrogel was directly contacted with BMSCs cells to determine the cytotoxicity of the hydrogel, such as Fig.11 As shown. The concentration range of nanoparticles was set at 2 μg / mL to 500 μg / mL. It was found that with the increase of nanoparticle concentration, the cell viability of BMSCs decreased. This was mainly because with the increase of nanoparticle concentration, the content of silver ions in the hydrogel also gradually increased. Silver ions would produce cytotoxicity to BMSCs cells, resulting in a decrease in BMSCs cell viability.
[0051] Antibacterial performance test: The antibacterial activity of piezoelectric composite hydrogel against Staphylococcus aureus was tested by the inhibition zone method. 50 μL of Staphylococcus aureus solution (10 6 CFU / mL) were evenly dispersed on the agar plate, the piezoelectric composite hydrogel was placed in a mold for solidification to obtain a hydrogel material with a diameter of 15 mm, the material was clamped with tweezers and placed on a plate, and ultrasonicated for 10 min respectively. The culture medium was placed in a carbon dioxide incubator at 37.5°C, and the diameter of the inhibition zone was measured after 24 h. The antibacterial performance of the hydrogel was evaluated by comparing the diameters of the inhibition zones. The diameter of the inhibition zone was the average of three parallel experiments. The results are shown in Table 1 below.
[0052] Group Inhibition zone diameter Example 1 33.61mm Comparative Example 1 32.54mm Comparative Example 2 19.83mm Comparative Example 3 29.52mm Antibacterial rate experiment: The piezoelectric composite hydrogel was placed in a mold for curing to obtain a hydrogel material with a diameter of 15 mm. The prepared piezoelectric composite hydrogel was added to a 12-well plate and 50 μL of Staphylococcus aureus solution (10 6 CFU / mL) was added to the surface of the piezoelectric composite hydrogel and placed in a 37°C constant temperature incubator for incubation for 6 hours; each experimental group was ultrasonically sonicated for 10 minutes, and 200 microliters of sterile PBS solution was added to each group of samples in turn to resuspend the bacteria. 50 microliters of bacterial suspension was evenly dispersed on the agar plate using the coating plate method and cultured at 37°C for 24 hours. After the culture was completed, the total number of bacteria was recorded and a blank control group was set. Inhibition rate = (number of colonies in the blank control group - number of colonies in the experimental group) / number of colonies in the blank control group × 100%. The value of the inhibition rate is the average of 3 parallel experiments. The numerical results are shown in Fig.12 .
[0053] Table 1 shows the experimental results of the in vitro antibacterial properties of the piezoelectric composite hydrogels of Example 1 and Comparative Example 1. Fig.12 The results of the antibacterial rate of the piezoelectric composite hydrogel in Example 1 and Comparative Example 1 are shown in Table 1 and Fig.12The data results show that the piezoelectric composite hydrogel in the present invention has excellent antibacterial effect. At the same time, compared with Example 1, the antibacterial activity and antibacterial rate of the piezoelectric composite hydrogels in Comparative Examples 1-3 are reduced. The above experimental results show that both carboxymethyl chitosan and Ag-BaTiO3 have antibacterial effects, and the two can effectively improve the antibacterial performance of the piezoelectric composite hydrogel together.
[0054] The piezoelectric composite hydrogel for promoting bone repair and the preparation method thereof of the present invention have the beneficial effects of: using GelMA hydrogel as a matrix, adding growth factors to induce the formation of new bone tissue by promoting the generation of extracellular matrix of bone cells, and adding piezoelectric Ag-BaTiO3 and positively charged carboxymethyl chitosan to effectively promote cell penetration and migration, and promote the regeneration of bone tissue together with the growth factors, thereby preparing Ag-BaTiO3 / CMCS / growth factor / piezoelectric composite hydrogel, while ensuring the overall performance of the composite hydrogel material, utilizing the piezoelectric properties of bone tissue and the self-powered characteristics of the piezoelectric material to establish an electric field in situ, thereby achieving the purpose of stimulating bone tissue regeneration.
[0055] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a piezoelectric composite hydrogel for promoting bone repair, It is characterized in that the steps include: (1) Nano-BaTiO 3 The powder is mixed with silver ammonia solution to obtain nano Ag-BaTiO 3 ; (2) Using carboxymethyl chitosan as a dispersant, nano-Ag-BaTiO 3 The piezoelectric composite hydrogel is obtained by mixing the piezoelectric composite hydrogel with transforming growth factor and adding the mixture to the gel precursor, and then adding a curing agent to cause a cross-linking reaction.
2. A method for preparing a piezoelectric composite hydrogel for promoting bone repair according to claim 1, It is characterized in that The nano BaTiO 3 The mass ratio of the powder to the silver ammonia solution is 1:20-40.
3. A method for preparing a piezoelectric composite hydrogel for promoting bone repair according to claim 1, It is characterized in that The carboxymethyl chitosan, the nano Ag-BaTiO 3 The mass ratio of the transforming growth factor to the transforming growth factor is 1:0.2-2:0.1-0.
5.
4. The method for preparing a piezoelectric composite hydrogel for promoting bone repair according to claim 1, It is characterized in that The growth factors include one or more of bone morphogenetic protein BMP, bone-derived growth factor BDGF, and growth transfer factor TGF-β1.
5. The method for preparing a piezoelectric composite hydrogel for promoting bone repair according to claim 1, It is characterized in that The gel precursor is a combination of one or more of methacrylated gelatin, carboxymethyl chitosan gel and polyvinyl alcohol gel.
6. A piezoelectric composite hydrogel for promoting bone repair and a preparation method thereof according to claim 1, It is characterized in that The carboxymethyl chitosan is prepared by subjecting chitosan to carboxymethylation reaction in alkali solution.
7. A piezoelectric composite hydrogel for promoting bone repair and a preparation method thereof according to claim 1, It is characterized in that The curing agent is an ultraviolet curing agent.
8. A piezoelectric composite hydrogel for promoting bone repair and a preparation method thereof according to claim 1, It is characterized in that The methacrylated gelatin is prepared by swelling gelatin, mixing it with methacrylic anhydride, and then dialyzing it.
9. A piezoelectric composite hydrogel for promoting bone repair, It is characterized in that Prepared by the preparation method described in any one of claims 1 to 8.
10. A piezoelectric composite hydrogel patch for promoting bone repair. It is characterized in that The invention comprises a piezoelectric composite hydrogel layer prepared by the preparation method according to any one of claims 1 to 8, and a backing layer and an isolation layer respectively arranged on two sides of the piezoelectric composite hydrogel layer.
Citation Information
Cited By
Piezoelectric / conductive integrated hydrogel for skull defect repair and application thereof
CN120078949A
A Piezoelectric / Conductive Integrated Hydrogel for Skull Defect Repair and Its Application
CN120078949B