Method for preparing ultramicro filter membrane by spraying segmented copolymer spherical micelles and ultramicro filter membrane
By spraying block copolymer spherical micelles on the surface of the macroporous base membrane to form an ultra-microfiltration membrane with a gradient structure, it solves the problems in the existing technology of difficulty in controlling the pore structure and difficulty in improving the flux selectivity of the separation process at the same time, and achieves ultra-microfiltration membranes. The adjustable pore size of the microfiltration membrane and the improvement of separation performance reduce the safety and environmental risks of the process.
Patent Information
- Application Number
- CN202410840497.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing ultra-microfiltration membrane preparation process has problems such as difficulty in controlling the pore structure and difficulty in simultaneously improving the flux and selectivity of the separation process. In addition, a large amount of organic solvents are used in the process, which poses safety and environmental risks.
By spraying block copolymer spherical micelles, block copolymer spherical micelles of different particle sizes are sequentially sprayed on the surface of the macroporous base membrane to form a separation layer with a gradient structure to prepare an ultramicrofiltration membrane.
It achieves the controllable pore size of ultra-microfiltration membrane, breaks through the trade off effect between flux and selectivity, reduces process safety and environmental risks, and improves the separation performance of the membrane.
Smart Images

Figure HDA0004914262910000011 
Figure HDA0004914262910000012 
Figure HDA0004914262910000021
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a composite ultrafiltration membrane, in particular to a method for preparing an ultrafiltration membrane by spraying block copolymer spherical micelles. Background Art
[0002] Membrane separation is a technology that uses membrane materials as media and achieves efficient separation of substances through the principle of selective permeability. Compared with other separation technologies, membrane separation has the outstanding advantages of high efficiency and energy saving. According to the size of the substances to be separated, membrane separation is divided into different application fields such as microfiltration, ultrafiltration, nanofiltration, reverse osmosis, and gas separation. Microfiltration and ultrafiltration are membrane separation technologies that were developed earlier. They are widely used and thus have a huge market. It is generally believed that the pore size ranges of microfiltration membranes and ultrafiltration membranes are ~0.1-10μm and ~2-100nm, respectively, but there is no strict limit to the pore size range of the two, and they are mainly prepared by wet phase conversion methods, so they are usually referred to as "ultra-microfiltration membranes". Microfiltration membranes and ultrafiltration membranes have the advantages of relatively large pore sizes, low working pressure differences (<0.5MPa), no phase change in the separation process, and low energy consumption. They have been widely used in water treatment processes such as wastewater treatment, reclaimed water reuse, and tap water production.
[0003] Although it has been widely used, the further development of ultrafiltration membranes also faces some bottleneck problems, which restricts the improvement of its application level and the expansion of its application field. Ultrafiltration membranes are mainly prepared by the process of phase transformation of polymer solutions in water. This is a macroscopic phase separation process. The phase separation process occurs randomly and disorderly. The process of generating a polymer-poor phase is the pore-forming process, which is easily affected by small dynamic disturbances, resulting in the discreteness of membrane pores in time and space. The polymer-poor phase is transformed into a pore channel, and phase separation and pore formation occur simultaneously. It is difficult to control the microstructure of the pore channel, and the pore size distribution of the obtained separation membrane is wide, resulting in the mutual restriction of flux and selectivity in the membrane separation process, and they cannot be improved at the same time. In addition, this process requires the use of a large amount of organic solvents and produces difficult-to-treat wastewater. Therefore, there are relatively serious safety risks, environmental risks and pollution risks in the phase transformation manufacturing process of ultrafiltration membranes.
[0004] Therefore, it is of great significance to invent a simple, efficient and controllable separation membrane pore size preparation method. Summary of the invention
[0005] The purpose of the present invention is to improve the deficiencies of the prior art and provide a simple and efficient method for preparing an ultramicrofiltration membrane based on block copolymer micelles.
[0006] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0007] In the first aspect, a method for preparing an ultrafiltration membrane by spraying block copolymer spherical micelles is provided, that is, using block copolymer spherical nano micelles as the membrane casting unit, spraying block copolymer micelles of different sizes on the surface of the macroporous base membrane in sequence to form a separation layer with a gradient structure, and preparing the ultrafiltration membrane; the specific steps are as follows:
[0008] a) placing the block copolymer in a selective solvent, and preparing at least two block copolymer spherical micelle solutions with different particle sizes by different heating induction methods;
[0009] b) spraying at least two block copolymer spherical micelle solutions with different particle sizes obtained in a) in order of particle size from large to small on the surface of the macroporous base membrane to obtain a composite membrane composed of micelle solutions with various particle sizes;
[0010] c) placing the composite film formed by spraying in step b) in air to dry naturally.
[0011] In a preferred embodiment of the present invention, the block copolymer described in a) consists of block A and block B, wherein block A is polysulfone and block B is polyethylene glycol; and the block A accounts for 30%-50% of the total volume percentage of the block copolymer.
[0012] In a preferred embodiment of the present invention, in the at least two block copolymer spherical micelle solutions with different particle sizes obtained in a), the particle sizes of the block copolymer spherical micelles are all between 30-600 nm; preferably between 30-300 nm; more preferably between 30-250 nm.
[0013] In a more preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes obtained in a) include two block copolymer spherical micelle solutions with an average particle size of 200-250nm and an average particle size of 30-100nm; in a further preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes obtained in a) include two block copolymer spherical micelle solutions with an average particle size of 250nm and an average particle size of 30-80nm.
[0014] In a preferred embodiment of the present invention, the selective solvent in step a) is acetic acid or ethanol; further preferably, the block copolymer is added to the acetic acid or ethanol to form a solution with a mass percentage concentration of 0.1%-3%.
[0015] In the scheme described in the present invention, the macroporous base membrane described in step b) is any membrane material that does not react with the selective solvent described in step a); preferably, the macroporous base membrane is a polyethersulfone membrane.
[0016] In the solution of the present invention, in the spraying described in step b), it is preferred to control the amount of the block copolymer spherical micelle solution in each spraying layer to be 0.16-0.28 mL / cm 2 Basement membrane.
[0017] In a more preferred embodiment, the spraying in b) is performed by a spray coating apparatus, and the spray coating apparatus is further preferably controlled to have a spraying pressure of 1 bar, a spraying height of 62 mm, and a spraying moving speed of 100 mm min. -1 .
[0018] In a second aspect, the present invention also provides an ultramicrofiltration membrane comprising a base layer, a support layer and a separation layer, wherein the support layer and the separation layer are formed by layered spraying and stepwise deposition of at least two block copolymer spherical micelle solutions with different particle sizes, and the order of the layered spraying is from large to small in terms of the particle size of the block copolymer spherical micelles.
[0019] In a preferred embodiment of the present invention, the block copolymer contained in the at least two block copolymer spherical micelle solutions with different particle sizes consists of block A and block B, wherein block A is polysulfone and block B is polyethylene glycol; and the block A accounts for 30%-50% of the total volume percentage of the block copolymer.
[0020] In a preferred embodiment of the present invention, in the at least two block copolymer spherical micelle solutions with different particle sizes, the particle sizes of the block copolymer spherical micelles are all between 30-600 nm; preferably between 30-300 nm; more preferably between 30-250 nm.
[0021] In a more preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes include two block copolymer spherical micelle solutions with an average particle size of 200-250nm and an average particle size of 30-100nm; in a further preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes include two block copolymer spherical micelle solutions with an average particle size of 250nm and an average particle size of 30-80nm; or include three block copolymer spherical micelle solutions with an average particle size of 250nm, an average particle size of 70-80nm and an average particle size of 25-35nm.
[0022] In a preferred embodiment of the present invention, the mass percentage concentration of the at least two block copolymer spherical micelle solutions with different particle sizes is 0.1%-3%.
[0023] In the solution described in the present invention, the base layer is any polyethersulfone membrane.
[0024] In summary, the present invention provides a process for preparing an ultrafiltration membrane: at least two block copolymer micelles are sprayed on the surface of a base membrane to form a structure in which micelles with large particle sizes serve as a support layer at the bottom and micelles with small particle sizes serve as a single-layer, double-layer or multi-layer gradient micelle separation layer at the top, and the ultrafiltration membrane is obtained by natural drying.
[0025] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in the following aspects:
[0026] (1) A new idea of using spray coating to prepare block copolymer micelle composite membranes was proposed. The method is simple and easy to operate;
[0027] (2) By using micelles of different particle sizes for stepwise deposition, the structure of the micelle support layer and the separation layer can be controlled to obtain a gradient pore structure, which is beneficial to break through the trade-off effect of membrane flux retention;
[0028] (3) The effective pore size of the prepared ultrafiltration membrane separation layer can be controlled by changing the particle size of the micelles, and the minimum molecular weight cutoff can be as low as 1493Da. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The SEM images of the block copolymer micelle composite membrane sprayed in Example 1 are shown in FIG. 1 , wherein (a) is a surface SEM image, and (b) is a cross-sectional SEM image.
[0030] Figure 2 The pure water flux of the ultrafiltration membrane prepared by spraying different volumes of micelles in Example 2 and the retention data of bovine serum albumin (BSA) and 50nm silica spheres are shown in Figure 2. 5+4 is a membrane prepared by 5mL of micelles with an average particle size of 250nm + 4mL of micelles with an average particle size of 75nm, and the same is true for 5+5, 5+6 and 5+7.
[0031] Figure 3 The pure water flux of the ultrafiltration membrane prepared by spraying different volumes of micelles in Example 3 and the retention data of bovine serum albumin (BSA) and lysozyme are shown in Figure 3. 3+3 is a membrane prepared by 3 mL of micelles with an average particle size of 250 nm + 3 mL of micelles with an average particle size of 30 nm, and the same is true for 3+2 and 3+1.
[0032] Figure 4 This is a molecular weight cutoff curve of the ultrafiltration membrane prepared by spraying different volumes of micelles in Example 3. 3+3 is a membrane prepared by 3 mL of micelles with an average particle size of 250 nm + 3 mL of micelles with an average particle size of 30 nm, and the same applies to 3+2 and 3+1. DETAILED DESCRIPTION
[0033] The present invention is further described below in conjunction with specific embodiments, but the given embodiments do not constitute a limitation on the saturation scope of the claims of the present invention.
[0034] Example 1
[0035] The method of preparing an ultramicrofiltration membrane having a double-layer micelle structure including a support layer and a single-layer separation layer by spraying block copolymer spherical micelles comprises the following steps:
[0036] a) adding polysulfone-polyethylene glycol to acetic acid at a mass fraction of 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer spherical micelle solution with an average particle size of 250 nm;
[0037] b) adding polysulfone-polyethylene glycol to ethanol with a mass fraction controlled at 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer spherical micelle solution with an average particle size of 30 nm;
[0038] c) Take a piece of polyethersulfone (PES) membrane (membrane area 25cm 2 ), place it under the sprayer and fix it;
[0039] d) 5 mL of a spherical micelle solution of a block copolymer of polysulfone and polyethylene glycol with a particle size of 250 nm was measured and sprayed on the surface of the polyethersulfone base membrane. The spray pressure of the sprayer was controlled to be 1 bar, the spray height to be 62 mm, and the spray moving speed to be 100 mm / min. -1 , forming the first micellar layer;
[0040] e) Measure 3 mL of a spherical micelle solution of a block copolymer of polysulfone and polyethylene glycol with a particle size of 30 nm and spray it on the surface of the polyethersulfone base membrane. Control the spray pressure of the sprayer to be 1 bar, the spray height to be 62 mm, and the spray moving speed to be 100 mm min -1 , forming the second micelle layer;
[0041] f) placing the spray-prepared ultrafine filtration membrane in air to dry naturally, thereby obtaining a three-layer ultrafine filtration membrane having PES as a base layer, large-size micelles as a support layer, and small-size micelles as a separation layer.
[0042] Depend on Figure 1 It can be seen that the block copolymer micelle composite membrane prepared in Example 1 has a smooth surface and uniform distribution of micelles, and the double-layer micelles in the cross section are clearly visible. The thickness of the small micelle layer that determines the separation performance is 202 nm.
[0043] Example 2
[0044] The method of preparing an ultramicrofiltration membrane having a double-layer micelle structure including a support layer and a single-layer separation layer by spraying block copolymer spherical micelles comprises the following steps:
[0045] a) adding polysulfone-polyethylene glycol to acetic acid at a mass fraction of 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer micelle solution with an average particle size of 250 nm;
[0046] b) adding polysulfone-polyethylene glycol to acetic acid with a mass fraction controlled at 0.1%, and heating the solution at 180° C. for 6 hours to obtain a block copolymer micelle solution with an average particle size of 75 nm;
[0047] c) Take a piece of polyethersulfone (PES) membrane (membrane area 25cm 2 ), place it under the sprayer and fix it;
[0048] d) measuring 5 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 250 nm, and spraying it on the surface of the polyethersulfone base membrane to form a first micelle layer;
[0049] e) 4 mL, 5 mL, 6 mL, and 7 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 75 nm were respectively measured and sprayed on the surface of the polyethersulfone base membrane to form a second micelle layer;
[0050] f) placing the spray-prepared ultrafine filtration membrane in air to dry naturally, thereby obtaining a three-layer ultrafine filtration membrane with PES as the base layer, large-size micelles as the support layer, and small-size micelles as the separation layer.
[0051] Depend on Figure 2 It can be seen that for the block copolymer micelle composite membrane prepared in Example 2, as the spraying amount of the second layer of micelles increased from 4 mL to 7 mL, the water flux of the ultrafiltration membrane gradually decreased from 87 to 69 L·m -2 ·h -1 bar -1 The retention of BSA increased from 4.5% to 9.8%, and the retention of SiO2 was about 50%. This is because with the increase of micelle spraying amount, the thickness of separation layer increased, which increased the mass transfer resistance of the membrane, resulting in a decrease in water flux and an increase in retention.
[0052] Example 3
[0053] The method of preparing an ultramicrofiltration membrane having a double-layer micelle structure including a support layer and a single-layer separation layer by spraying block copolymer spherical micelles comprises the following steps:
[0054] a) adding polysulfone-polyethylene glycol to acetic acid at a mass fraction of 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer micelle solution with an average particle size of 250 nm;
[0055] b) adding polysulfone-polyethylene glycol to ethanol with a mass fraction controlled at 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer micelle solution with an average particle size of 30 nm;
[0056] c) Take a piece of polyethersulfone (PES) membrane (membrane area 25cm 2 ), place it under the sprayer and fix it;
[0057] d) measuring 3 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 250 nm, and spraying it on the surface of the polyethersulfone base membrane to form a first micelle layer;
[0058] e) measuring 3 mL, 2 mL, and 1 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 30 nm, respectively, and spraying them on the surface of the polyethersulfone base membrane to form a second micelle layer;
[0059] f) placing the spray-prepared ultrafine filtration membrane in air to dry naturally, thereby obtaining a three-layer ultrafine filtration membrane with PES as the base layer, large-size micelles as the support layer, and small-size micelles as the separation layer.
[0060] Depend on Figure 3 It can be seen that for the block copolymer micelle composite membrane prepared in Example 3, when the spraying amount of the second layer of micelles was 3 mL, 2 mL, and 1 mL, the water flux of the ultrafiltration membrane was 15, 17, and 170 L·m, respectively. -2 ·h -1 bar -1 The retention rates of BSA were 98%, 96% and 11% respectively, and the retention rates of lysozyme were 98%, 97% and 13% respectively.
[0061] Depend on Figure 4 It can be seen that when 3 mL 250 nm + 3 mL 30 nm micelles are used to construct the micelle layer, the ultrafiltration membrane prepared in Example 3 has a minimum molecular weight cutoff of 1493 Da.
[0062] Example 4
[0063] The method of preparing an ultramicrofiltration membrane having a three-layer micelle structure including a support layer and a double-layer separation layer by spraying block copolymer spherical micelles comprises the following steps:
[0064] a) adding polysulfone-polyethylene glycol to acetic acid at a mass fraction of 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer micelle solution with an average particle size of 250 nm;
[0065] b) adding polysulfone-polyethylene glycol to acetic acid with a mass fraction controlled at 0.1%, and heating the solution at 180° C. for 6 hours to obtain a block copolymer micelle solution with an average particle size of 75 nm;
[0066] c) adding polysulfone-polyethylene glycol to ethanol with a mass fraction controlled at 0.1%, and heating the solution at 180° C. for 12 hours to obtain a block copolymer micelle solution with an average particle size of 30 nm;
[0067] d) Take a piece of polyethersulfone (PES) membrane (membrane area of 25 cm2) and place it under the sprayer and fix it;
[0068] e) measuring 3 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 250 nm, and spraying it on the surface of the polyethersulfone base membrane to form a first micelle layer;
[0069] f) measuring 2 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 75 nm, and spraying it on the surface of the polyethersulfone base membrane to form a second micelle layer;
[0070] g) measuring 1 mL of a polysulfone-polyethylene glycol block copolymer micelle solution with a particle size of 30 nm, and spraying it on the surface of the polyethersulfone base membrane to form a third micelle layer;
[0071] h) The ultrafiltration membrane prepared by spraying is placed in the air to dry naturally, so as to obtain a multilayer micellar ultrafiltration membrane with PES as the base layer, 250nm large particle size micelles as the support layer, and 75nm+30nm small particle size micelles as the double-layer separation layer.
Claims
1. A method for preparing an ultramicrofiltration membrane by spraying block copolymer spherical micelles, characterized in that: The following steps are involved: a) placing the block copolymer in a selective solvent, and preparing at least two block copolymer spherical micelle solutions with different particle sizes by different heating induction methods; b) spraying at least two block copolymer spherical micelle solutions with different particle sizes obtained in a) on the surface of the macroporous base membrane in descending order of the particle size of the block copolymer spherical micelle; A composite membrane consisting of micelle solutions with various particle sizes is obtained; c) placing the composite film formed by spraying in step b) in air to dry naturally.
2. The method according to claim 1, characterized in that: a) The block copolymer is composed of block A and block B, wherein block A is polysulfone and block B is polyethylene glycol; and the block A accounts for 30%-50% of the total volume percentage of the block copolymer.
3. The method according to claim 1, characterized in that: a) In the at least two block copolymer spherical micelle solutions with different particle sizes obtained, the particle sizes of the block copolymer spherical micelles are all between 30-600nm; preferably, they are all between 30-250nm; in a more preferred embodiment, a) The at least two block copolymer spherical micelle solutions with different particle sizes obtained include two block copolymer spherical micelle solutions with an average particle size of 200-250nm and an average particle size of 30-100nm; in a further preferred embodiment, a) The at least two block copolymer spherical micelle solutions with different particle sizes obtained include two block copolymer spherical micelle solutions with an average particle size of 250nm and an average particle size of 30-80nm.
4. The method according to claim 1, characterized in that: The selective solvent described in a) is acetic acid or ethanol; further preferably, the block copolymer is added to the acetic acid or ethanol to form a solution with a mass percentage concentration of 0.1%-3%.
5. The method according to claim 1, characterized in that: The macroporous base membrane described in b) is any membrane material that does not react with the selective solvent described in a); preferably, the macroporous base membrane is a polyethersulfone membrane.
6. The method according to claim 1, characterized in that: b) In the spraying, the amount of the block copolymer spherical micelle solution in each spraying layer is controlled to be 0.16-0.28 mL / cm 2 Basement membrane.
7. The method according to claim 1, characterized in that: b) The spraying is completed by a spraying apparatus, and the spraying pressure of the spraying apparatus is controlled to be 1 bar, the spraying height is 62 mm, and the spraying moving speed is 100 mm min -1 .
8. An ultra-microfiltration membrane comprising a base layer, a support layer and a separation layer, characterized in that: The support layer and the separation layer are formed by layered spraying and stepwise deposition of at least two block copolymer spherical micelle solutions with different particle sizes. The order of layered spraying is from large to small according to the particle size of the block copolymer spherical micelle.
9. The ultramicrofiltration membrane according to claim 8, characterized in that: The block copolymer contained in the spherical micelle solution of at least two block copolymers with different particle sizes consists of block A and block B, wherein block A is polysulfone and block B is polyethylene glycol; and the block A accounts for 30%-50% of the total volume percentage of the block copolymer.
10. The ultramicrofiltration membrane according to claim 8, characterized in that: In the at least two block copolymer spherical micelle solutions with different particle sizes, the particle sizes of the block copolymer spherical micelles are all between 30-600nm; preferably, they are all between 30-250nm; in a more preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes include two block copolymer spherical micelle solutions with an average particle size of 200-250nm and an average particle size of 30-100nm; in a further preferred embodiment, the at least two block copolymer spherical micelle solutions with different particle sizes include two block copolymer spherical micelle solutions with an average particle size of 250nm and an average particle size of 30-80nm.
11. The ultramicrofiltration membrane according to claim 8, characterized in that: The mass percentage concentration of the at least two block copolymer spherical micelle solutions with different particle sizes is 0.1%-3%.
12. The ultramicrofiltration membrane according to claim 8, characterized in that: The base layer is a polyethersulfone membrane.
Citation Information
Patent Citations
Method for preparing porous membrane based on segmented copolymer fibre micel
CN103120903A
Preparation method and use of spiropyrane group-containing diblock copolymer
CN103910838A
Preparation method of polymeric micelle nanofiltration membrane and application thereof
CN108654409A
Microwave-enhanced selective swelling pore-forming method for separation membrane
CN110124539A
Method for producing a separating membrane and separating membrane that can be produced by said method
EP3056260A1