Preparation method of super-hydrophobic super-oleophylic flame-retardant polyurethane sponge and application of super-hydrophobic super-oleophylic flame-retardant polyurethane sponge in oil-water separation

Through the preparation of modified polyurethane sponge materials, the problem of absorption capacity and repeatability of adsorbent materials in oil-water separation is solved, and the hydrophobicity and flame retardant properties of the material are improved through modification treatment, achieving efficient oil-water separation and environmentally friendly oil-water separation effect.

CN118767887AActive Publication Date: 2024-10-15CHANGZHOU UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410808487.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing adsorbent materials have problems with low oil recovery, poor absorption capacity, non-selective absorption and difficulty in reuse in oil-water separation, and polyurethane sponges are limited by their hydrophilicity and flammability.

Method used

By modifying polyurethane sponge with materials such as cobalt nitrate hexahydrate, 2-methylimidazole, zinc nitrate hexahydrate and PDMS, a super-hydrophobic and super-oleophilic flame-retardant polyurethane sponge is prepared, using a non-toxic, harmless, simple and environmentally friendly method process to form efficient oil-water separation materials.

Benefits of technology

It achieves high saturated oil absorption capacity, oil-water separation efficiency and flame retardant performance. It has good mechanical properties and cycle adsorption capacity, low cost, non-toxic and harmless materials, and is green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767887A_ABST
    Figure CN118767887A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of functional materials, and particularly relates to a preparation method of super-hydrophobic super-oleophylic flame-retardant polyurethane sponge and application of the super-hydrophobic super-oleophylic flame-retardant polyurethane sponge in oil-water separation. The preparation method comprises the following steps: dispersing a proper amount of prepared nickel-cobalt hydrotalcite (NiCo-LDH) and ZIF-8 into a PDMS (Polydimethylsiloxane) diluent to form a dispersion liquid, soaking the polyurethane sponge into the dispersion liquid, stirring for a period of time, taking out, and drying. The super-hydrophobic, super-oleophylic and flame-retardant efficient oil-water separation sponge material is prepared through a dipping method, the hydrophobic angle can reach 153.4 degrees, the combustion time can be prolonged to 16 s from original 5 s, the saturated oil absorption can reach 26.6-82.9 times of the self, and after 20 times of adsorption-extrusion circulation, the composite sponge can still reach the super-hydrophobic state.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional materials, and particularly relates to a preparation method of a super-hydrophobic and super-oleophilic flame-retardant polyurethane sponge and an application of the sponge in oil-water separation. Background Art

[0002] With the rapid development of modern science and technology, the pollution problems caused by industrialization to the environment need to be paid more and more attention, especially oil spill treatment, chemical leakage and organic waste liquid discharge have posed a serious threat to the ecosystem, and usually cause dangers such as fire and explosion. A large number of mammals and seabirds will continue to be harmed, causing irreparable harm to human life and health. Therefore, it is very necessary to find a reliable, effective and environmentally friendly oil spill treatment method.

[0003] People have developed some new materials and methods to achieve effective oil-water separation, including adsorption, dispersion, in-situ combustion, skimming, bioremediation, chemical dispersion, filtration, etc., but most of these methods are time-consuming and labor-intensive, and may even cause secondary pollution to the environment. Among them, adsorption is low-cost and green and environmentally friendly, and is a more recommended method for removing oil and organic pollutants from water. However, traditional adsorption materials (such as cotton fabric, zeolite, activated carbon, fly ash, etc.) used to remove oil compounds and organic pollutants from water have almost all kinds of disadvantages, including low oil recovery, poor absorption capacity, non-selective absorption and difficulty in reuse. Therefore, the preparation of adsorbents with excellent superhydrophobic / superoleophilic surfaces is crucial for oil-water separation.

[0004] New three-dimensional (3D) porous materials are widely used in oil-water separation due to their high adsorption capacity, simple preparation, environmental friendliness and low price. Such materials include polystyrene sponge (PS), polyurethane sponge (PU), polyvinyl alcohol sponge (PVA) and melamine sponge (MS). Among them, PU sponge can be used as an ideal adsorption material considering its advantages such as light weight, low cost, large specific surface area, high porosity and good adsorption repeatability. However, PU sponge is hydrophilic and flammable and will produce toxic gases after being ignited, which greatly limits their application. Summary of the invention

[0005] In order to solve the problems pointed out in the background technology part, the present invention provides a simple, environmentally friendly and easy-to-operate method to prepare a super-hydrophobic and super-oleophilic flame-retardant polyurethane sponge with high adsorption capacity, good separation efficiency and high reuse rate. In order to solve the above technical problems, the technical solution adopted by the present invention includes the following steps:

[0006] (1) Cut the commercially available polyurethane sponge into 1×1×1 cm 3The blocks were ultrasonically cleaned with anhydrous ethanol and deionized water for 30 min each, and then placed in an oven for drying.

[0007] (2) 3 g of cobalt nitrate hexahydrate and 4 g of 2-methylimidazole were dissolved in 100 mL of anhydrous methanol, and then the mixture was stirred for 20 min and allowed to stand for 24 h. The solution after standing was centrifuged, and then washed with anhydrous methanol and dried in a vacuum drying oven at 35° C. to obtain ZIF-67;

[0008] (3) 0.5 g ZIF-67 was dissolved in 200 mL anhydrous ethanol by ultrasonication for 20 min, and 1.35 g nickel nitrate hexahydrate was added, stirred on a magnetic stirrer for 40 min, transferred to an 80 ° C oil bath for incubation for 48 h, centrifuged, washed with deionized water and anhydrous ethanol three times each, and dried at 35 ° C to obtain NiCo-LDH;

[0009] (4) 1.488 g of zinc nitrate hexahydrate and 1.642 g of 2-methylimidazole were dissolved in anhydrous methanol by stirring for 20 min respectively, and then the two solutions were mixed and stirred on a magnetic stirrer for 2 h. After standing for 6 h, they were centrifuged and washed with anhydrous methanol for 3 times each, and freeze-dried to obtain ZIF-8;

[0010] (5) Dissolve PDMS and curing agent in 40 mL of n-hexane by ultrasonic for 30 min, add appropriate amount of NiCo-LDH in step (3) and ZIF-8 in step (4) and ultrasonically dissolve for 30 min, then add PU cleaned in step (1), stir on a magnetic stirrer (speed of 180 rpm) for 50 min, take out the sponge and put it into a 120 ° C oven to dry for 4 h to obtain a super hydrophobic and super oleophilic flame retardant polyurethane sponge;

[0011] Among them, the mass ratio of PDMS, curing agent, NiCo-LDH and ZIF-8 is: 1:0.1:0.25-1:0.25-1.

[0012] Compared with the prior art, the present invention has the following advantages:

[0013] 1. The super-hydrophobic modification process of the present invention is simple, convenient, low-cost, and the main raw materials are non-toxic and harmless, and are green and environmentally friendly.

[0014] 2. The prepared modified superhydrophobic sponge has excellent saturated oil absorption capacity, oil-water separation efficiency and flame retardant properties.

[0015] 3. The hydrophobic, oleophilic, flame-retardant sponge prepared by the present invention has good mechanical properties and cyclic adsorption capacity, and can maintain its original appearance and adsorption performance after repeated extrusion and recycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1This is a comparison chart of the hydrophobic angle, burning time, and saturated oil absorption data for n-hexane and chloroform of the sponges prepared in Examples 1-7 of the present invention.

[0017] Figure 2 FESEM images of PU and NiCo-LDH / ZIF-8-PDMS-PU prepared in Example 1 of the present invention.

[0018] Figure 3 (a) and (b) are state diagrams of water droplets and oil droplets falling on the original sponge and NiCo-LDH / ZIF-8-PDMS-PU surfaces in Example 1 of the present invention, respectively; (c) a state diagram of water droplets on the cross-section of NiCo-LDH / ZIF-8-PDMS-PU; (d) a state diagram of the original sponge in water and NiCo-LDH / ZIF-8-PDMS-PU floating on water; (e) a state diagram of the silver mirror phenomenon of NiCo-LDH / ZIF-8-PDMS-PU under water;

[0019] Figure 4 This is a time comparison chart of the combustion conditions of the original PU and NiCo-LDH / ZIF-8-PDMS-PU in Example 1 of the present invention.

[0020] Figure 5 This is a data graph of the saturated absorption of NiCo-LDH / ZIF-8-PDMS-PU to various oils / organic reagents in Example 1 of the present invention.

[0021] Figure 6 This is a graph showing the hydrophobic angle data of NiCo-LDH / ZIF-8-PDMS-PU in Example 1 of the present invention after being immersed in different salt concentrations for 12 hours.

[0022] Figure 7 This is a data graph of the hydrophobic angle of NiCo-LDH / ZIF-8-PDMS-PU in Example 1 of the present invention after being immersed in different pH conditions for 12 hours. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with embodiments, but is not limited thereto.

[0024] 1. Oil / organic solution absorption capacity test

[0025] The oil absorption performance of the prepared NiCo-LDH / ZIF-8-PDMS-PU was tested by soaking it in various oils / organic solvents (such as petroleum ether, n-hexane, n-octane, heavy oil, tetrahydrofuran, benzene, toluene, dichloromethane, and chloroform) for 5 minutes. First, the NiCo-LDH / ZIF-8-PDMS-PU was weighed as m1, immersed in 20 mL of oil or organic solvent for 5 minutes, and the sponge was taken out and weighed as m2. The saturated absorption capacity of the sponge was expressed as QS It can be calculated by the following formula:

[0026] Q S =(m2-m1) / m1

[0027] All test results require the average value of three samples to ensure data accuracy.

[0028] 2. Oil-water separation efficiency and reusability test

[0029] The reusability of NiCo-LDH / ZIF-8-PDMS-PU was tested by repeated absorption-extrusion cycles. The mass of the sponge before oil absorption was recorded as m1. The sponge was immersed in oil or organic solvent at ambient temperature for 5 minutes to make the sponge saturated with absorption. The mass of the sponge at this time was recorded as m2. The saturated sponge was placed in a syringe and the syringe was manually pushed to compress the sponge until all the oil adsorbed by the sponge was squeezed out and no oil droplets were separated. The mass of the sponge after desorption was recorded as m3 and used for the next cycle. The cycle was repeated 1-10 times, and the mass of the sponge before and after oil absorption and desorption was recorded in each cycle.

[0030] The first saturated oil absorption rate is recorded as k a,1 , k a,1 =[(m2-m1) / m1]×100%

[0031] The nth saturated oil absorption rate is recorded as k a,n , k a,n =[(m 3n-1 -m 3n-2 ) / m 3n-2 ]×100%

[0032] The first separation efficiency is recorded as η, that is, η = (m2-m3) / (m2-m1)

[0033] The nth separation efficiency is denoted as η n , that is, η n =(m 3n-1 -m 3n ) / (m 3n-1 -m 3n-2 )

[0034] 3. Environmental stability test

[0035] Soak NiCo-LDH / ZIF-8-PDMS-PU in acid-base solutions with pH=1, 3, 5, 7, 9, 11, and 13 for 12 hours, take out the sponge, rinse it with anhydrous ethanol, dry it, and measure the water contact angle. Soak NiCo-LDH / ZIF-8-PDMS-PU in NaCl solutions with concentrations of 1.5%, 2.5%, 3.5%, 4.5%, and 5.5% for 12 hours, take out the sponge, rinse it with anhydrous ethanol, dry it, and measure the water contact angle.

[0036] Example 1

[0037] (1) Cut the commercially available polyurethane sponge into 1×1×1 cm 3 The blocks were ultrasonically cleaned with anhydrous ethanol and deionized water for 30 min each, and then placed in an oven for drying.

[0038] (2) 3 g of cobalt nitrate hexahydrate and 4 g of 2-methylimidazole were added to 100 mL of anhydrous methanol respectively, stirred for 20 min to dissolve, and solution A and solution B were obtained. Solution A was quickly added to solution B, stirred for 20 min, and then allowed to stand for 24 h. The solution after standing was centrifuged, and then washed with anhydrous methanol for 3 times and placed in a vacuum drying oven at 35°C to obtain ZIF-67; 0.5 g of ZIF-67 was added to 200 mL of anhydrous ethanol, ultrasonicated for 20 min, and then 1.35 g of nickel nitrate hexahydrate was added. After stirring for 40 min, the mixture was incubated at 80°C for 2 days. After centrifugation, the mixture was washed with deionized water and anhydrous ethanol for 3 times in sequence, and placed in a vacuum drying oven at 35°C to obtain NiCo-LDH;

[0039] (3) 1.488 g of zinc nitrate hexahydrate and 1.642 g of 2-methylimidazole were added to 100 mL of anhydrous methanol, respectively, and stirred for 20 min to obtain solution A and solution B. Solution A was added to solution B, stirred for 2 h, allowed to stand for 6 h, and then centrifuged. The solution was then washed three times with anhydrous methanol and freeze-dried to obtain ZIF-8.

[0040] (4) Add 0.5 g of polydimethylsiloxane with vinyl active groups (Dow Corning PDMS) and 0.05 g of curing agent (polydimethylsiloxane with hydrogen groups, Dow Corning Sylgard 184) into 40 mL of n-hexane, and ultrasonicate for 30 min. Then, add 0.25 g of NiCo-LDH and 0.25 g of ZIF-8 and ultrasonicate for 30 min. Then, add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it into an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0041] Example 2

[0042] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0043] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0044] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0045] (4) Add 0.25 g PDMS and 0.025 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.125 g NiCo-LDH and 0.125 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0046] Example 3

[0047] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0048] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0049] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0050] (4) Add 0.75 g PDMS and 0.075 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.325 g NiCo-LDH and 0.325 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0051] Example 4

[0052] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0053] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0054] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0055] (4) 1 g PDMS and 0.1 g curing agent were added to 40 mL n-hexane, and ultrasonicated for 30 min. Then, 0.5 g NiCo-LDH and 0.5 g ZIF-8 were added and ultrasonicated for 30 min. Then, the cleaned PU was added and stirred at 180 rpm for 50 min. The sponge was taken out and dried in an oven at 120 °C for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0056] Example 5

[0057] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0058] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0059] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0060] (4) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.125 g NiCo-LDH and 0.125 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0061] Example 6

[0062] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0063] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0064] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0065] (4) 0.5 g PDMS and 0.05 g curing agent were added to 40 mL n-hexane, and ultrasonicated for 30 min. Then, 0.325 g NiCo-LDH and 0.325 g ZIF-8 were added and ultrasonicated for 30 min. Then, the cleaned PU was added and stirred at 180 rpm for 50 min. The sponge was taken out and dried in an oven at 120 °C for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0066] Example 7

[0067] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0068] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0069] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0070] (4) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.5 g NiCo-LDH and 0.5 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0071] Example 8

[0072] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0073] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0074] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0075] (4) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.375 g NiCo-LDH and 0.125 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0076] The burning time is 15s, the hydrophobic angle is 152.3°, the oil absorption of chloroform is 78.5234g / g, and the oil absorption of n-hexane is 25.3284g / g.

[0077] Example 9

[0078] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0079] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0080] (3) The preparation steps of ZIF-8 are the same as those in Example 3;

[0081] (4) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, then add 0.125 g NiCo-LDH and 0.375 g ZIF-8 and ultrasonicate for 30 min. Add the cleaned PU and stir at 180 rpm for 50 min. Take out the sponge and put it in an oven at 120 °C to dry for 4 h to obtain NiCo-LDH / ZIF-8-PDMS-PU.

[0082] The burning time is 14.5s, the hydrophobic angle is 151.8°, the oil absorption of chloroform is 76.3258g / g, and the oil absorption of n-hexane is 25.1032g / g.

[0083] Comparative Example 1

[0084] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0085] (2) The preparation steps of NiCo-LDH are the same as those in Example 2;

[0086] (3) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, add 0.5 g NiCo-LDH and ultrasonicate for 30 min, add the cleaned PU, stir at 180 rpm for 50 min, take out the sponge and put it in a 120 °C oven to dry for 4 h to obtain NiCo-LDH-PDMS-PU.

[0087] The burning time is 14s, the hydrophobic angle is 150.3°, the oil absorption of chloroform is 72.2589g / g, and the oil absorption of n-hexane is 23.4561g / g.

[0088] Comparative Example 2

[0089] (1) The sponge cleaning preparation steps are the same as in Example 1;

[0090] (2) The preparation steps of ZIF-8 are the same as those in Example 3;

[0091] (3) Add 0.5 g PDMS and 0.05 g curing agent to 40 mL n-hexane, ultrasonicate for 30 min, add 0.5 g ZIF-8 and ultrasonicate for 30 min, add the cleaned PU, stir at 180 rpm for 50 min, take out the sponge and put it in a 120 °C oven to dry for 4 h to obtain ZIF-8-PDMS-PU.

[0092] The burning time is 14s, the hydrophobic angle is 151.4°, the oil absorption of chloroform is 73.5741g / g, and the oil absorption of n-hexane is 23.8657g / g.

Claims

1. A method for preparing a super-hydrophobic and super-oleophilic flame-retardant polyurethane sponge, characterized in that: The preparation method steps are as follows: (1) Cut the polyurethane sponge into 1×1×1cm 3 The blocks were ultrasonically cleaned with anhydrous ethanol and deionized water in turn, and placed in an oven for drying. (2) dissolving cobalt nitrate hexahydrate and 2-methylimidazole in anhydrous methanol respectively, then mixing and stirring and letting stand, centrifuging the solution after standing, washing with anhydrous methanol and drying in a vacuum drying oven to obtain ZIF-67; (3) dissolving ZIF-67 in anhydrous ethanol by ultrasonication, adding nickel nitrate hexahydrate, stirring on a magnetic stirrer, transferring to an oil bath for incubation, centrifuging, washing with deionized water and anhydrous ethanol in sequence, and drying to obtain NiCo-LDH; (4) zinc nitrate hexahydrate and 2-methylimidazole are stirred and dissolved in anhydrous methanol respectively, and then the two solutions are mixed and stirred on a magnetic stirrer, allowed to stand and then centrifuged, washed with anhydrous methanol, and freeze-dried to obtain ZIF-8; (5) ultrasonically dissolving PDMS and a curing agent in n-hexane, adding the NiCo-LDH in step (3) and the ZIF-8 in step (4) and ultrasonically dissolving them, then adding the PU cleaned in step (1), stirring on a magnetic stirrer, taking out the sponge and putting it into an oven to dry, thereby obtaining a super hydrophobic and super oleophilic flame retardant polyurethane sponge.

2. The method for preparing a super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, wherein: When preparing ZIF-67 in step (2), the mass ratio of cobalt nitrate hexahydrate to 2-methylimidazole is 3:4, the amount of anhydrous methanol is 100 mL, the stirring time after mixing is 20 min, the standing time is 24 h, and the vacuum drying temperature is 35 ° C.

3. The preparation method of super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, characterized in that: When preparing NiCo-LDH in step (3), the mass ratio of ZIF-67 to nickel nitrate hexahydrate is 1:2.7, and the ultrasonic dissolution time is 20 min.

4. The preparation method of super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, characterized in that: In step (3), the stirring time is 40 min, the incubation time in the oil bath is 48 h, the temperature is 80° C., washing is performed 3 times, and the drying temperature is 35° C.

5. The preparation method of super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, characterized in that: When preparing ZIF-8 in step (4), the mass ratio of zinc nitrate hexahydrate to 2-methylimidazole is 1.488:1.642, the stirring time after mixing is 2 hours, the standing time is 6 hours, and washing is performed 3 times.

6. The preparation method of super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, characterized in that: In step (5), the mass ratio of PDMS, curing agent, NiCo-LDH and ZIF-8 is: 1:0.1:0.25-1:0.25-1.

7. The preparation method of super hydrophobic and super oleophilic flame retardant polyurethane sponge as claimed in claim 1, characterized in that: In step (5), the ultrasonic time is 30 min, the stirring time is 50 min, the rotation speed is 180 rpm, the drying temperature is 120° C., and the time is 4 h.

8. A super hydrophobic and super oleophilic flame retardant polyurethane sponge prepared by the method according to any one of claims 1 to 7.

9. An application of a super hydrophobic and super oleophilic flame retardant polyurethane sponge prepared by the method according to any one of claims 1 to 7, characterized in that: The polyurethane sponge is used for oil-water separation.

Citation Information

Patent Citations

  • Preparation method of nickel-cobalt layered bimetallic hydroxide / graphene electrocatalyst

    CN107824188A

  • Oil-water separated super-hydrophobic foam preparation method

    CN108854160A

  • PNT@NiCo-LDH composite material applied to supercapacitor and preparation method of PNT@NiCo-LDH composite material

    CN111933455A

  • Preparation method of CCO / CoNiMn-LDH composite material and application of CCO / CoNiMn-LDH composite material in super capacitor

    CN113299484A

  • Amphibious hydrophobic-oleophylic finishing agent and application thereof in dye adsorption and separation

    CN114892403A