Composite catalyst as well as preparation method and application thereof

By growing doped titanium dioxide nanoparticles on an inorganic carrier to prepare a composite catalyst, it solves the problems of solid acid catalyst reusability and insufficient catalyst life, achieving efficient and low-cost biodiesel preparation and improving raw material adaptability.

CN118767906APending Publication Date: 2024-10-15SINOPEC SHANGHAI ENGINEERING CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310382654.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, the reusability and catalyst life of solid acid catalysts are insufficient, resulting in high biodiesel preparation costs and difficulty in effectively utilizing animal and vegetable oil raw materials with complex compositions.

Method used

Using inorganic carriers (such as kaolin) as the substrate, doped titanium dioxide nanoparticles are grown through the solution-gel method to prepare composite catalysts, improve catalytic activity and recycling rate, and reduce catalyst dosage and production costs.

Benefits of technology

It achieves a catalyst with high catalytic activity and long life, reduces the cost of biodiesel preparation, improves raw material adaptability and process efficiency, reduces purification and refining steps, and is suitable for the preparation of complex raw materials such as kitchen waste grease and dairy residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767906A_ABST
    Figure CN118767906A_ABST
Patent Text Reader

Abstract

The invention discloses a composite catalyst as well as a preparation method and application thereof. The composite catalyst comprises an inorganic carrier and metal element doped titanium dioxide loaded on the inorganic carrier. The method comprises the following steps: uniformly mixing acid and a titanium source in a solvent to prepare a titanium source solution; dispersing an inorganic carrier in water to prepare powder slurry; uniformly mixing the titanium source solution, the powder slurry and the metal salt solution, aging to obtain particles, and calcining the dried particles to obtain the composite catalyst. The composite catalyst disclosed by the invention can show relatively high catalytic activity in the transesterification reaction, and the catalyst is low in dosage and high in repeated utilization rate. When the composite catalyst provided by the invention is used for preparing biodiesel, complex purification and refining steps can be avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomass energy chemical industry, and more particularly to a composite catalyst and a preparation method and application thereof. Background Art

[0002] Biodiesel refers to a liquid fuel that can replace fossil diesel and is made from animal and plant oils and waste oils through an ester exchange process. Compared with petrochemical diesel, the combustion products of biodiesel are more non-toxic and less harmful to the environment. With the increasing environmental protection requirements, biodiesel can be used as a new environmentally friendly energy source to replace petrochemical diesel.

[0003] At present, the main methods for preparing biodiesel are acid catalysis and base catalysis. Among them, the acid catalysis method for preparing biodiesel can be divided into liquid acid catalysis and solid acid catalysis. Commonly used liquid acid catalysts include sulfuric acid, phosphoric acid, hydrochloric acid, nitric acid, etc. Although liquid acid catalysis has high efficiency, it also has many disadvantages, such as the danger of large-dose transportation and storage, long-term operation is highly corrosive to equipment, difficult to separate and purify for recycling, and acid mist tail gas is prone to environmental pollution. Compared with liquid acid catalysts, although the cost price of solid acid catalysts is slightly higher, solid acid catalysts have high catalytic efficiency, can be recovered, regenerated, and recycled, the prepared product is simple to post-process, and has low corrosion to equipment. Therefore, for the large-scale preparation of biodiesel, solid acid catalysts have great industrial advantages and have become a hot spot for research and development in the industry.

[0004] However, in the prior art, the reusability of solid acid catalysts for preparing biodiesel needs to be further improved. It is necessary to continue to increase the catalyst life and reduce the amount of catalyst added, thereby reducing production costs. In addition, it is also necessary to improve the universality of the process for raw materials and better apply it to the preparation of biodiesel from raw materials with complex ingredients such as waste cooking oil and dairy residues, such as animal and plant oils.

[0005] Therefore, it is necessary to prepare a solid acid catalyst with better performance. Summary of the invention

[0006] In order to solve the problems in the prior art, the present invention proposes a composite catalyst and a preparation method and application thereof. The present invention uses an inorganic carrier (such as natural mineral kaolin) as a catalyst raw material, and in situ grows metal-doped titanium dioxide nanoparticles on the surface by a solution-gel method to prepare a composite nanocatalyst. Because the metal-doped titanium dioxide nanoparticles have a unique high surface area and active sites, the catalyst can show a high catalytic activity in the transesterification reaction, and the catalyst dosage is low and the reuse rate is high. The biodiesel preparation process can also avoid complex purification and refining steps.

[0007] In order to solve the above problems, the present invention proposes the following technical solutions:

[0008] One of the purposes of the present invention is to provide a composite catalyst, which comprises an inorganic carrier and titanium dioxide doped with a metal element supported on the inorganic carrier.

[0009] In the composite catalyst of the present invention, preferably,

[0010] The metal element doped in the titanium dioxide is selected from non-transition metal elements, preferably, the non-transition metal element is selected from at least one of zinc, cobalt, nickel and zirconium;

[0011] The inorganic carrier is selected from at least one of kaolin, clay and bentonite.

[0012] In the composite catalyst of the present invention, preferably,

[0013] The mass ratio of the metal element-doped titanium dioxide to the inorganic carrier is 2% to 8%, preferably 3% to 7%; and / or,

[0014] In the titanium dioxide doped with metal elements, the content of the metal elements is 3% to 10% of the mass of the titanium dioxide, preferably 3% to 7%.

[0015] In the composite catalyst of the present invention, preferably,

[0016] The specific surface area of ​​the composite catalyst is 300-500m 2 / g; and / or,

[0017] The pore volume of the composite catalyst is 0.40-0.80 cm 2 / g; and / or,

[0018] The particle size of the composite catalyst is 4400-5900 meshes.

[0019] The second object of the present invention is to provide a method for preparing a composite catalyst, comprising the following steps:

[0020] (1) mixing an acid and a titanium source uniformly in a solvent to prepare a titanium source solution; dispersing an inorganic carrier in water to prepare a slurry;

[0021] (2) mixing the titanium source solution and the slurry, adding the metal salt solution and mixing evenly, aging to obtain particles, and calcining the dried particles to obtain a composite catalyst;

[0022] It is preferably used to prepare the composite catalyst described in any one of the purposes of the present invention.

[0023] In the method for preparing the composite catalyst of the present invention, preferably,

[0024] The acid is selected from at least one of phosphoric acid and organic acid; preferably, the organic acid is selected from at least one of glacial acetic acid, oxalic acid and citric acid; and / or,

[0025] The titanium source is selected from at least one of organic titanates and titanium salts; preferably, the organic titanate is selected from at least one of tetrabutyl titanate and tetraisopropyl titanate; and / or, the titanium salt is selected from at least one of titanium tetrachloride and titanyl sulfate; and / or,

[0026] The solvent is selected from an alcohol solvent, preferably, the alcohol solvent is selected from at least one of methanol, ethanol, isopropanol, ethylene glycol, and n-butanol; and / or,

[0027] The concentration of the titanium source in the solvent is 20-30 wt %; and / or,

[0028] The volume of the acid added is 0.5%-2% of the total volume of the titanium source dissolved in the solvent; preferably, the acid is added after the titanium source and the solvent.

[0029] In the method for preparing the composite catalyst of the present invention, preferably,

[0030] In the slurry, the particle size of the inorganic carrier is 4500-6000 mesh; and / or,

[0031] The solid-liquid ratio is maintained at 0.1Kg / L-0.5Kg / L;

[0032] Preferably, the inorganic carrier is crushed, ground, washed, filtered, pulped with water, and pulverized to obtain a slurry; further preferably, the inorganic carrier is simply crushed, pressed into a coarse powder below 500 mesh, washed once with 10 times the mass ratio of water, filtered, and then the solid powder is sent to a slurry barrel, water is added, stirred and pulped, and ultrafinely ground to 4500-6000 mesh using a vertical mill, and the solid-liquid ratio is maintained at 0.1Kg / L-0.5Kg / L.

[0033] In the method for preparing the composite catalyst of the present invention, preferably,

[0034] The volume of the titanium source solution added is 5%-20% of the volume of the slurry, preferably 5%-10%; and / or,

[0035] The metal salt in the metal salt solution is selected from at least one of chlorides of non-metallic transition elements and sulfates of non-metallic transition elements; preferably selected from at least one of zinc chloride, zinc sulfate, cobalt chloride, cobalt sulfate, nickel chloride, nickel sulfate, zirconium chloride and zirconium sulfate; the metal elements in the metal salt solution are doped into titanium dioxide as doping elements; and / or,

[0036] The concentration of the metal salt solution is 5-10wt%; the volume of the metal salt solution added is 0.5%-2% of the volume of the slurry, preferably 0.5%-1%; and / or,

[0037] The aging time is 12-24 hours; and / or,

[0038] The calcination temperature is 390-490°C; the calcination time is 30-40 minutes.

[0039] More preferably, after the titanium source solution and the slurry are mixed, the metal salt solution is added and mixed evenly; and / or,

[0040] After aging, the particles are filtered, dried, and then calcined. In the present invention, the drying temperature after aging can be selected from the commonly used temperature, preferably the drying temperature is 50-70°C; the drying time is 6-12h;

[0041] The third object of the present invention is to provide a composite catalyst as described in any one of the first objects of the present invention or a composite catalyst prepared by the preparation method as described in any one of the second objects of the present invention in the preparation of biodiesel; preferably,

[0042] The oil-containing raw material, the cosolvent, the composite catalyst and at least one of the C1-C2 alcohols are mixed and subjected to transesterification reaction to obtain biodiesel; preferably, after the transesterification reaction is completed, the reaction is allowed to stand, the upper phase after standing is taken, filtered and washed with water, and the upper clear liquid is taken and distilled and dried to obtain purified biodiesel.

[0043] In the present invention, the catalyst is recovered through the filter cake solid, and can be reused after washing and drying.

[0044] The crude biodiesel (crude biodiesel after esterification reaction) in the existing conventional biodiesel contains residual fatty acids, residual water, proteins, polysaccharides and other pigments, colloidal or greasy impurities, which need to be decolorized with activated carbon and washed with water multiple times. The polar surface and porous loose structure of the composite catalyst of the present invention can replace the activated carbon, reduce the amount and number of water washings, and avoid complicated purification and refining steps.

[0045] In the method for preparing the composite catalyst of the present invention, preferably,

[0046] The oil-containing raw material is selected from at least one of vegetable oil, animal oil, waste oil, microbial oil, and dairy residue; and / or

[0047] The co-solvent is selected from at least one of petroleum ether, n-hexane, n-pentane, n-heptane, ethyl ether, methyl tert-butyl ether, acetone and chloroform; and / or,

[0048] The C1-C2 alcohol is selected from at least one of methanol and ethanol.

[0049] In the method for preparing the composite catalyst of the present invention, preferably,

[0050] The amount of the composite catalyst added is 1%-5% of the mass of the oil-containing raw material; preferably 1%-2.5%; and / or,

[0051] The amount of the co-solvent added is 10-40% of the volume of the C1-C2 alcohol; preferably 10-20%; and / or,

[0052] In the present invention, the higher the acid content of the oil-containing raw material, the greater the proportion of the C1-C2 alcohol used; preferably, the volume ratio of the oil-containing raw material to the C1-C2 alcohol is 1:5-1:20; more preferably, 1:5-1:10;

[0053] The temperature of the transesterification reaction is 40-80°C; preferably 40-60°C; and / or,

[0054] The transesterification reaction time is 6 to 24 hours, preferably 10 to 16 hours.

[0055] The present invention utilizes a solution gel method to in-situ grow nano titanium dioxide particles on the surface of an inorganic carrier, and utilizes active metal elements to dope the titanium dioxide particles to further increase catalytic active sites and improve the catalytic efficiency of the catalyst. In the present invention, the inorganic carrier does not require complicated treatment, and only the inorganic carrier is ground and refined, and the generation of nano titanium dioxide and the doping of active substances are simultaneously achieved by a "one-pot method", and the prepared powder is aged and calcined to obtain a composite nano catalyst, and the process is simple and fast.

[0056] In addition, the present invention uses an inorganic carrier, especially a natural mineral such as kaolin, as a substrate, which can not only provide pores as a catalyst carrier, but also has a certain catalytic activity itself, so that the prepared catalyst has better activity; and the inorganic carrier itself does not require complicated process treatment, which can effectively reduce the energy consumption and material consumption of the catalyst preparation process, greatly reduce the production cost, and has good economic and technical advantages when applied to biodiesel preparation, and can be better applied to industrial production and replacement of petrochemical diesel.

[0057] Finally, the present invention also greatly enhances the compatibility of the alcohol and oil phases by adding an organic co-solvent in the ester exchange reaction, increases the contact area between the alcohol and oil phases, reduces the mass transfer resistance between the alcohol and oil phases, promotes the oil molecules to enter the methanol solution from the solid or oil phase interface, and enables the oil in the oil to be quickly dissolved in the alcohol. Therefore, under the action of the composite catalyst of the present invention, the ester exchange reaction can occur under relatively low temperature conditions, and a relatively high yield of biodiesel can be obtained in a relatively short time.

[0058] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0059] Compared with the prior art, the present invention has at least the following beneficial technical effects:

[0060] 1) The composite catalyst of the present invention has high catalytic activity and long catalyst life, and has good technical advantages;

[0061] 2) When the composite catalyst of the present invention is used to prepare biodiesel, it has wide adaptability to raw oils and fats, low reaction temperature and short reaction time;

[0062] 3) The composite catalyst of the present invention has a small amount of addition, a high recycling rate, and a low price of inorganic carrier, which greatly reduces the production cost and has excellent economic adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 This is a graph showing the effect of reaction time on ester exchange conversion rate during the preparation of biodiesel in the present invention;

[0064] Figure 2 This is a graph showing the effect of reaction temperature on ester exchange conversion rate during the preparation of biodiesel in the present invention. DETAILED DESCRIPTION

[0065] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0066] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0067] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0068] The following are the raw materials used in the examples:

[0069] Kaolin: Kaolin ore raw soil, particle size 325 mesh, was purchased from Shengfei Mineral Products Processing Plant in Lingshou County, Shijiazhuang City.

[0070] Titanate: industrial grade, purchased from Zhuhai Weiken Chemical Co., Ltd.

[0071] The following are various embodiments of the method for preparing the catalyst of the present invention:

[0072] Example 1

[0073] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of zinc chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0074] Example 2

[0075] Prepare 1L of 20% by mass titanium sulfate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of zinc chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0076] Example 3

[0077] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of cobalt chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0078] Example 4

[0079] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of nickel chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0080] Example 5

[0081] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural white clay powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of zinc chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0082] Example 6

[0083] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed bentonite powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of zinc chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0084] Example 7

[0085] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution and 100mL of zirconium chloride aqueous solution (5wt%), stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 450℃ for 30 minutes, and cool at room temperature to obtain the catalyst.

[0086] The composition and content of the composite catalyst prepared in the above examples are shown in Table 1 below:

[0087] Table 1

[0088]

[0089] The specific surface area of ​​the composite catalysts prepared in the above examples is 300-500m 2 / g; the pore volume of the composite catalyst is between 0.40-0.80cm 2 / g; the particle size of the composite catalyst is between 4400-5900 mesh.

[0090] Comparative Example 1

[0091] Prepare 1L of 20% by mass tetrabutyl titanate ethanol solution, add 20mL of glacial acetic acid, stir evenly for use, and prepare a titanium source solution; then send 1Kg of washed natural kaolin powder into a slurry barrel, add 10L of water, stir and slurry, use a vertical mill to ultrafinely grind to 4500-6000 mesh, and prepare a slurry; then add 1L of titanium source solution, stir at room temperature for 2h, stop stirring, age for 24h, then filter through a filter press, dry at 70℃ for 12h, and then send to a calcining furnace for calcination at a temperature of 390-490℃ for 30 minutes, and cool at room temperature to obtain a catalyst.

[0092] Comparative Example 2

[0093] 1 kg of washed natural kaolin powder is placed in a slurry barrel, 10 L of water is added, stirred and slurried, and ultrafinely ground to 4500-6000 mesh using a vertical mill to obtain a slurry; then 100 mL of a zinc chloride aqueous solution (5 wt%) is added, stirred at room temperature for 2 hours, stirring is stopped, aged for 24 hours, and then filtered through a filter press and dried at 70°C for 12 hours, and then sent to a calcining furnace for calcination at a temperature of 390-490°C for 30 minutes, and cooled at room temperature to obtain the catalyst.

[0094] Example 8

[0095] The present invention further provides a method for preparing biodiesel, comprising the following steps:

[0096] 10 kg of waste catering oil is mixed with petroleum ether, a catalyst and methanol for transesterification reaction, the volume ratio of raw oil to methanol is 1:5-1:10, the co-solvent petroleum ether is 10% of the volume of methanol, and the amount of the composite catalyst used is 1%-2.5% of the mass fraction of the raw oil. After reacting at 40-60° C. for 12 hours, the mixture is allowed to stand, and the lower phase is filtered to recover the catalyst solid; the upper phase after standing is taken, filtered and washed with water, and the upper clear liquid is taken for distillation and drying to obtain biodiesel. The catalyst is the catalyst prepared in the aforementioned embodiments and comparative examples respectively.

[0097] Test method:

[0098] The product was analyzed by gas chromatography using a GC-2010 gas chromatograph (Shimadzu, Japan), a DB1-ht capillary column (0.25 mm × 30 m, Agilient), high-purity nitrogen as carrier gas, a hydrogen flame ionization detector, a detector temperature of 375 ° C, and a vaporization chamber temperature of 370 ° C. The methyl ester content of the transesterification product was measured to determine the biodiesel yield. The specific results are shown in Table 2.

[0099] Table 2

[0100]

[0101] It can be seen from the data in Table 2 that, compared with the comparative example, the yield of biodiesel prepared in Examples 1 to 7 is higher, indicating that the nanocomposite catalyst of the present invention has high catalytic activity and strong selectivity; and the biodiesel conversion rate of the kaolin sample is higher than that of the clay and bentonite samples, indicating that kaolin is the most preferred; from the comparison of various conditions in Example 1, it can be found that the increase in temperature, catalyst dosage, and alcohol-to-oil ratio has little effect on the conversion rate. At 40°C, 1% catalyst dosage, and 1:5 alcohol-to-oil ratio, a conversion rate of more than 95% can be achieved under a reaction time of 12h, while the influence of temperature, catalyst dosage, and alcohol-to-oil ratio on the conversion rate in the comparative example is more significant, indicating that the production process of biodiesel adopted in the embodiment has the characteristics of low energy consumption and low material consumption.

[0102] Figure 1 The figure is the effect of reaction time on biodiesel conversion rate during the preparation of biodiesel in the embodiments of the present invention and the comparative examples. In the embodiment 1, 90% biodiesel conversion rate can be obtained in 6 hours, and the reaction reaches equilibrium after 12 hours, and the conversion rate no longer increases. The biodiesel conversion rates of comparative examples 1 and 2 need to reach equilibrium after 16-24 hours, and the conversion rates are between 85-90%. The data show that the embodiments have higher biodiesel conversion rate and efficiency than the comparative examples.

[0103] Figure 2 The figure is a test chart of the biodiesel cyclic conversion performance of the embodiment of the present invention. The catalyst is tested for the number of times it can be reused in the biodiesel preparation system. After each reaction, the solid catalyst can be filtered out of the filtrate, washed with water, and dried, and can be used again in the transesterification reaction. The conversion rate of biodiesel is measured under the same reaction conditions. The results are shown in Figure 2 As shown, after the composite catalysts of various embodiments were reused for 30 times, the residual conversion rate was above 85%, indicating that the catalysts had strong catalytic activity and could be reused repeatedly.

[0104] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

[0105] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.

[0106] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0107] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.

Claims

1. A composite catalyst, Features: The composite catalyst comprises an inorganic carrier and titanium dioxide doped with a metal element supported on the inorganic carrier.

2. The composite catalyst according to claim 1, Features: The metal element doped in the titanium dioxide is selected from non-transition metal elements, preferably, the non-transition metal element is selected from at least one of zinc, cobalt, nickel and zirconium; and / or, The inorganic carrier is selected from at least one of kaolin, clay and bentonite.

3. The composite catalyst according to claim 1, Features: The mass ratio of the metal element-doped titanium dioxide to the inorganic carrier is 2% to 8%, preferably 3% to 7%; and / or, In the titanium dioxide doped with metal elements, the content of the metal elements is 3% to 10% of the mass of the titanium dioxide, preferably 3% to 7%.

4. The composite catalyst according to claim 1, Features: The specific surface area of ​​the composite catalyst is 300-500m 2 / g; and / or, The pore volume of the composite catalyst is 0.40-0.80 cm 2 / g; and / or, The particle size of the composite catalyst is 4400-5900 meshes.

5. A method for preparing a composite catalyst, It is characterized in that The following steps are involved: (1) mixing an acid and a titanium source uniformly in a solvent to prepare a titanium source solution; dispersing an inorganic carrier in water to prepare a slurry; (2) uniformly mixing the titanium source solution, the slurry and the metal salt solution, aging to obtain particles, and calcining the dried particles to obtain a composite catalyst; It is preferably used to prepare the composite catalyst according to any one of claims 1 to 4.

6. The method for preparing the composite catalyst according to claim 5, Features: Step (1), The acid is selected from at least one of phosphoric acid and organic acid; preferably, the organic acid is selected from at least one of glacial acetic acid, oxalic acid and citric acid; and / or, The titanium source is selected from at least one of organic titanates and titanium salts; preferably, the organic titanate is selected from at least one of tetrabutyl titanate and tetraisopropyl titanate; and / or, the titanium salt is selected from at least one of titanium tetrachloride and titanyl sulfate; and / or, The solvent is selected from an alcohol solvent, preferably, the alcohol solvent is selected from at least one of methanol, ethanol, isopropanol, ethylene glycol, and n-butanol; and / or, The concentration of the titanium source in the solvent is 20-30 wt %; and / or, The volume of the acid added is 0.5%-2% of the total volume of the titanium source dissolved in the solvent.

7. The method for preparing the composite catalyst according to claim 5, Features: Step (1), In the slurry, the particle size of the inorganic carrier is 4500-6000 mesh; and / or, The solid-liquid ratio is maintained at 0.1Kg / L-0.5Kg / L.

8. The method for preparing the composite catalyst according to claim 5, Features: The volume of the titanium source solution added is 5%-20% of the volume of the slurry, preferably 5%-10%; and / or, The metal salt in the metal salt solution is selected from at least one of chlorides of non-metallic transition elements and sulfates of non-metallic transition elements; preferably selected from at least one of zinc chloride, zinc sulfate, cobalt chloride, cobalt sulfate, nickel chloride, nickel sulfate, zirconium chloride and zirconium sulfate; and / or, The concentration of the metal salt solution is 5-10wt%; the volume of the metal salt solution added is 0.5%-2% of the volume of the slurry, preferably 0.5%-1%; and / or, The aging time is 12-24 hours; and / or, The calcination temperature is 390-490°C; the calcination time is 30-40 minutes; More preferably, after the titanium source solution and the slurry are mixed, the metal salt solution is added and mixed evenly.

9. Use of the composite catalyst according to any one of claims 1 to 4 or the composite catalyst prepared by the preparation method according to any one of claims 5 to 8 in the preparation of biodiesel; preferably, The oil-containing raw material, a co-solvent, a composite catalyst and at least one of C1-C2 alcohols are mixed evenly to carry out a transesterification reaction to prepare biodiesel.

10. The use according to claim 9, Features: The oil-containing raw material is selected from at least one of vegetable oil, animal oil, waste oil, microbial oil, and dairy residue; and / or The co-solvent is selected from at least one of petroleum ether, n-hexane, n-pentane, n-heptane, ethyl ether, methyl tert-butyl ether, acetone and chloroform; and / or, The C1-C2 alcohol is selected from at least one of methanol and ethanol.

11. The use according to claim 9, Features: The amount of the composite catalyst added is 1%-5% of the mass of the oil-containing raw material; preferably 1%-2.5%; and / or, The amount of the co-solvent added is 10-40% of the volume of the C1-C2 alcohol; preferably 10-20%; and / or, The volume ratio of the oil-containing raw material to the C1-C2 alcohol is 1:5-1:20; preferably 1:5-1:10; The temperature of the transesterification reaction is 40-80°C; preferably 40-60°C; and / or, The transesterification reaction time is 6 to 24 hours, preferably 10 to 16 hours.

Citation Information

Patent Citations

  • Method of manufacturing biological diesel oil from hogwash oil

    CN101012388A

  • In-situ conversion method for simultaneously preparing biodiesel and animal feed by taking animal wastes as raw materials

    CN111471528A

  • Method for preparing synthesizing biodiesel oil solid acid catalyst by non-water solvent

    CN1911511A