Copper-zinc-magnesium-aluminum catalyst as well as precursor, preparation method and application thereof
Through the use of copper, zinc, magnesium and aluminum catalysts, the problems of expensive starting materials and catalyst deactivation in the preparation of long carbon chain ketones have been solved, and efficient and low-cost preparation of 2,6,8-trimethyl-4-nonanone has been achieved. , taking into account high conversion rate and high selectivity.
Patent Information
- Application Number
- CN202410825881.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
AI Technical Summary
When preparing long-carbon chain ketones in the prior art, the starting materials are expensive and require strict reaction conditions, resulting in high costs. In addition, the presence of impurities during the hydrogenation synthesis process causes catalyst deactivation, making separation difficult and affecting conversion rate and selectivity.
The copper-zinc-magnesium-aluminum catalyst is used to form a stable zinc-aluminum spinel structure to improve impurity resistance and high-temperature stability, and the rubber antioxidant production waste liquid is directly used to prepare 2,6,8-trimethyl in the presence of impurities. -4-Nonanone, achieving high conversion rate and high selectivity.
It improves the raw material conversion rate and product selectivity, reduces production costs, maintains catalyst activity in the presence of impurities, and improves the efficiency of industrial applications.
Smart Images

Figure CN118767923A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a copper-zinc-magnesium-aluminum catalyst and a precursor, a preparation method and an application thereof. Background Art
[0002] Branched-chain ketones are an important chemical raw material. Due to their special physical and chemical properties, they are widely used in daily chemical and industrial lubricant fields. Usually, the starting materials used for most long-chain ketones are relatively expensive compounds and are often prepared under strict reaction conditions and / or through necessary complex product separation steps, resulting in high costs for long-chain ketones, which is not conducive to industrial application. 2,6,8-trimethyl-4-nonanone, as a long-chain branched-chain ketone, is mainly used as a dispersant for vinyl chloride resins, a solvent for synthetic resin stabilizers, and a raw material for producing surfactants. Patent CN107935830B discloses a Ni-M / Al2O3 catalyst for catalyzing the one-step synthesis of 2,6,8-trimethyl-4-nonanone from methyl isobutyl ketone. It is prepared by an impregnation method. In an intermittent reactor, the reaction pressure is 1-5 MPa, the reaction temperature is 100-150°C, and the catalytic reaction is 3-8 hours. The conversion rate of methyl isobutyl ketone can reach up to 50%, and the selectivity of 2,6,8-trimethyl-4-nonanone is 90%.
[0003] Rubber antioxidant 6PPD is one of the general antioxidant varieties with excellent performance among amine antioxidant varieties. The production method of antioxidant 6PPD mainly adopts hydrogenation synthesis of p-aminodiphenylamine and methyl isobutyl ketone under the action of catalyst. This method has a short process flow and easy-to-obtain raw materials. It is the main method for industrial production of antioxidant 6PPD at home and abroad. However, in the hydrogenation synthesis process, part of methyl isobutyl ketone (MIBK) is hydrogenated to produce methyl isobutyl carbinol (MIBC), and the waste liquid contains a small amount of impurities such as alkanes with 3 to 9 carbons (including cycloalkanes and straight-chain alkanes), olefins with 3 to 9 carbons (including cycloolefins and straight-chain olefins) and amine compounds with benzene rings. The presence of impurities seriously affects the raw material conversion rate and product selectivity. Some impurities are poisons to the catalyst and easily lead to rapid deactivation of the catalyst. Since the physicochemical properties of MIBK, MIBC and other impurities are similar, it is difficult to separate them by distillation, and the energy consumption of refining MIBC and MIBK is high. Therefore, it is of great significance to use the waste liquid rich in MIBC and MIBK generated in the production process of industrial rubber antioxidant 6PPD as raw material directly to prepare high value-added 2,6,8-trimethyl-4-nonanone without refining treatment. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a copper-zinc-magnesium-aluminum catalyst and its precursor, preparation method and application. The copper-zinc-magnesium-aluminum catalyst of the present invention is used in the reaction of preparing 2,6,8-trimethyl-4-nonanone, with high raw material conversion rate and high product selectivity. Even if the waste liquid produced by the rubber antioxidant 6PPD is directly used as a raw material without refining treatment, it can be directly prepared into high value-added 2,6,8-trimethyl-4-nonanone in the presence of impurities, and high raw material conversion rate and high product selectivity can be guaranteed.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The present invention provides a copper-zinc-magnesium-aluminum catalyst precursor, which comprises a component A and a component B; the composition of the component A is expressed as ZnO-Al2O3; the composition of the component B is expressed as CuO-MgO-Al2O3; wherein,
[0007] The component A exists in a zinc-aluminum spinel structure;
[0008] In the component A, the molar ratio of Zn to Al is (0.10-1):1;
[0009] In the component B, the molar ratio of Cu and Mg elements is (0.10-1.01):1.
[0010] In the present invention, the active components are effectively isolated by forming a stable zinc-aluminum spinel structure through component A, which not only improves the catalyst's ability to resist impurities, but also helps to improve the high-temperature stability of the catalyst.
[0011] Preferably, the component A is distributed in the component B. Herein, "the component A is distributed in the component B" means that the component A is dispersed in the component B, and may also mean that the component A is the core and the component B is the shell, but it is not limited thereto.
[0012] In the present invention, in the component A, the molar ratio of Zn to Al is preferably (0.30-1):1, for example, 0.49:1, 0.50:1, 0.61:1 or 0.81:1.
[0013] In the present invention, in the component B, the molar ratio of Cu and Mg elements is preferably (0.10-0.80):1, more preferably (0.10-0.50):1; in the component B, the molar ratio of Cu and Mg elements is, for example, 0.13:1, 0.24:1, 0.29:1, 0.33:1, 0.48:1 or 0.63:1.
[0014] In the present invention, in the component B, the molar ratio of the sum of the molar numbers of Cu and Mg elements to the molar ratio of Al element is preferably (0.50-6):1, more preferably (1-5):1; in the component B, the molar ratio of the sum of the molar numbers of Cu and Mg elements to Al element is, for example, 1.05:1, 1.98:1, 2.55:1, 3.01:1, 3.36:1 or 3.58:1, 5.65:1 or 5.87:1.
[0015] In the present invention, the molar ratio of Al element in the component A and the component B is preferably (0.60-2):1, for example, 0.98:1 or 1:1.
[0016] In the present invention, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu and Al elements is preferably (0.14-1.14):1, for example, 0.15:1, 0.21:1, 0.25:1, 0.29:1, 0.56:1, 0.64:1 or 1.13:1.
[0017] In the present invention, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Zn to Al elements is preferably (0.23-0.40):1, for example, 0.25:1.
[0018] In the present invention, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Mg to Al elements is preferably (0.51-2.58):1, for example, 0.64:1, 0.74:1, 1.15:1, 1.21:1, 1.58:1 or 1.80:1.
[0019] In some preferred embodiments, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu and Al elements is (0.14-1.14):1; the molar ratio of Zn and Al elements is (0.23-0.40):1; and the molar ratio of Mg and Al elements is (0.51-2.58):1.
[0020] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.25:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 0.74:1.
[0021] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.29:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 1.21:1.
[0022] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.56:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 1.15:1.
[0023] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.21:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 1.58:1.
[0024] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.25:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 2.58:1.
[0025] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.64:1; the molar ratio of Zn to Al elements is 0.25:1; and the molar ratio of Mg to Al elements is 0.64:1.
[0026] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 0.15:1; the molar ratio of Zn to Al elements is 0.23:1; and the molar ratio of Mg to Al elements is 0.51:1.
[0027] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is 1.13:1; the molar ratio of Zn to Al elements is 0.40:1; and the molar ratio of Mg to Al elements is 1.80:1.
[0028] In the present invention, the content of CuO in the copper-zinc-magnesium-aluminum catalyst precursor is preferably 10%-40%, for example, 10.1%, 11.1%, 11.6%, 16.2%, 16.3%, 16.7%, 27.3%, 34.5% or 36.6%, where the percentage is the mass percentage of CuO in the copper-zinc-magnesium-aluminum catalyst precursor.
[0029] In the present invention, the content of ZnO in the copper-zinc-magnesium-aluminum catalyst precursor is preferably 5%-20%, for example, 10.5%, 12.5%, 13.3%, 13.4%, 13.6%, 14.2%, 16.9% or 18.2%, where the percentage is the mass percentage of ZnO in the copper-zinc-magnesium-aluminum catalyst precursor.
[0030] In the present invention, the content of MgO in the copper-zinc-magnesium-aluminum catalyst precursor is preferably 17%-60%, for example, 17.4%, 20.1%, 24.7%, 28.6%, 29.4%, 34.1%, 41.9% or 53.3%, where the percentage is the mass percentage of MgO in the copper-zinc-magnesium-aluminum catalyst precursor.
[0031] In the present invention, the content of Al2O3 in the copper-zinc-magnesium-aluminum catalyst precursor is preferably 15%-55%, for example, 20.7%, 26.2%, 31.6%, 33.6%, 34.5%, 35.5%, 42.1% or 50.1%, where the percentage is the mass percentage of Al2O3 in the copper-zinc-magnesium-aluminum catalyst precursor.
[0032] In some preferred embodiments, the CuO content is 10%-40%, the ZnO content is 5%-20%, the MgO content is 17%-60%, and the Al2O3 content is 15%-55%, wherein the percentages are the mass percentages of the components in the copper-zinc-magnesium-aluminum catalyst precursor.
[0033] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 16.3%, the content of ZnO is 16.9%, the content of MgO is 24.7%, and the content of Al2O3 is 42.1%.
[0034] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 16.2%, the content of ZnO is 14.2%, the content of MgO is 34.1%, and the content of Al2O3 is 35.5%.
[0035] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 27.3%, the content of ZnO is 12.5%, the content of MgO is 28.6%, and the content of Al2O3 is 31.6%.
[0036] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 11.1%, the content of ZnO is 13.4%, the content of MgO is 41.9%, and the content of Al2O3 is 33.6%.
[0037] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 10.1%, the content of ZnO is 10.5%, the content of MgO is 53.3%, and the content of Al2O3 is 26.2%.
[0038] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 34.5%, the content of ZnO is 13.6%, the content of MgO is 17.4%, and the content of Al2O3 is 34.5%.
[0039] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 11.6%, the content of ZnO is 18.2%, the content of MgO is 20.1%, and the content of Al2O3 is 50.1%.
[0040] In a specific embodiment, in the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 36.6%, the content of ZnO is 13.3%, the content of MgO is 29.4%, and the content of Al2O3 is 20.7%.
[0041] The present invention provides a method for preparing a copper-zinc-magnesium-aluminum catalyst precursor, which comprises the following steps:
[0042] S1. Performing a first precipitation reaction on a first precipitant aqueous solution and a first metal salt aqueous solution to obtain a mixed solution; wherein the first metal salt aqueous solution comprises a zinc salt and an aluminum salt; in the first metal salt aqueous solution, the molar ratio of Zn to Al is (0.10-1):1; the temperature of the first precipitation reaction is 40-80°C; and the endpoint pH value of the first precipitation reaction is 6-8;
[0043] S2, adding a second metal salt aqueous solution and a second precipitant aqueous solution to the mixed solution to carry out a second precipitation reaction; wherein the second metal salt aqueous solution comprises copper salt, magnesium salt and aluminum salt; the temperature of the second precipitation reaction is 40-80° C.; the endpoint pH value of the second precipitation reaction is 8-11; in the second metal salt aqueous solution, the molar ratio of Cu and Mg elements is (0.10-1.01):1;
[0044] S3, after post-treatment, the product is obtained; wherein the post-treatment includes roasting; the roasting temperature is 300-500°C.
[0045] In some preferred embodiments, in step S1, the first precipitant aqueous solution is first added to the reaction device, and then the first metal salt aqueous solution is added.
[0046] In some preferred embodiments, in step S1, the first metal salt aqueous solution is first added to the reaction device, and then the first precipitant aqueous solution is added.
[0047] In some other preferred embodiments, in step S1, the first metal salt aqueous solution and the first precipitant aqueous solution are added to the reaction device simultaneously.
[0048] Wherein, the above-mentioned reaction device can be a reaction kettle.
[0049] In some preferred embodiments, in step S2, the adding method is to sequentially add the second precipitant aqueous solution and the second metal salt aqueous solution into the mixed solution.
[0050] In some preferred embodiments, in step S2, the adding method is to sequentially add the second metal salt aqueous solution and the second precipitant aqueous solution into the mixed solution.
[0051] In some other preferred embodiments, in step S2, the adding method is to add the second metal salt aqueous solution and the second precipitant aqueous solution into the mixed solution at the same time.
[0052] In step S1, the metal salt in the first metal salt aqueous solution refers to a soluble metal salt conventionally used in the art, preferably including one or more of nitrate, chlorate, sulfate and acetate. The first metal salt aqueous solution refers to an aqueous solution of the above-mentioned soluble metal salt conventionally used in the art.
[0053] In step S2, the metal salt in the second metal salt aqueous solution refers to a soluble metal salt conventionally used in the art, preferably including one or more of nitrate, chlorate, sulfate and acetate. The second metal salt aqueous solution refers to an aqueous solution of the soluble metal salt conventionally used in the art.
[0054] In step S1, the concentration of the metal salt in the first metal salt aqueous solution is preferably 0.2-4 mol / L, for example, 0.50 mol / L, 0.60 mol / L, 0.65 mol / L, 0.71 mol / L, 0.74 mol / L, 0.80 mol / L, 0.94 mol / L or 1 mol / L.
[0055] In step S2, the concentration of the metal salt in the second metal salt aqueous solution is preferably 0.2-4 mol / L, for example, 0.90 mol / L, 1 mol / L or 1.1 mol / L.
[0056] In step S1, the precipitant in the first precipitant aqueous solution can be a soluble alkaline substance conventionally used in the art, preferably including one or more of K2CO3, Na2CO3, NaOH, NaHCO3 and KOH. The first precipitant aqueous solution refers to an aqueous solution of the soluble alkaline substance conventionally used as a precipitant in the art.
[0057] In step S2, the precipitant in the second precipitant aqueous solution can be a soluble alkaline substance conventionally used in the art, preferably including one or more of K2CO3, Na2CO3, NaOH, NaHCO3 and KOH. The second precipitant aqueous solution refers to an aqueous solution of the soluble alkaline substance conventionally used as a precipitant in the art.
[0058] In step S1, the mass fraction of the precipitant in the first precipitant aqueous solution is preferably 5%-30%, for example, 10%, 12% or 16%.
[0059] In step S2, the mass fraction of the precipitant in the second precipitant aqueous solution is preferably 5%-30%, for example, 13%, 13.1% or 18%.
[0060] In step S2, in the second metal salt aqueous solution, the molar ratio of the sum of the molar numbers of Cu and Mg elements to the Al element is (0.50-6):1; preferably (1-5):1; in the component B, the molar ratio of the sum of the molar numbers of Cu and Mg elements to the Al element is, for example, 1.05:1, 1.98:1, 2.55:1, 3.01:1, 3.36:1, 3.58:1, 5.65:1 or 5.87:1.
[0061] In step S1 and step S2, the molar ratio of Al element in the first metal salt aqueous solution and the second metal salt aqueous solution is (0.60-2):1, for example, 0.98:1 or 1:1.
[0062] In step S1, the temperature of the first precipitation reaction is preferably 40-70°C, for example 50°C.
[0063] In step S2, the temperature of the second precipitation reaction is preferably 40-70°C, for example 50°C.
[0064] In step S1, the endpoint pH value of the first precipitation reaction is preferably 6.5-7.5, for example 7.
[0065] In step S2, the endpoint pH value of the second precipitation reaction is preferably 8.5-10, for example 9 or 9.5.
[0066] In step S1, after the first precipitation reaction is completed, an aging step is preferably further included, wherein the aging temperature is preferably 40-70° C., such as 50° C., and the aging time is preferably 0.5-1 h.
[0067] In step S3, the calcination temperature is preferably 350-450°C, for example 400°C.
[0068] In step S3, the calcination time is preferably 0.5-4 h, for example 2 h or 4 h.
[0069] In step S3, in the post-treatment, preferably, aging, washing, filtering and drying are further performed before the calcination.
[0070] The aging can be performed by conventional methods in the art. The aging time is preferably 0.5-6 hours, such as 1 hour, 2 hours or 4 hours; the aging temperature is preferably 40-80°C, such as 50°C, 70°C or 75°C.
[0071] The washing can be carried out by conventional methods in the art. The detergent used in the washing is preferably deionized water.
[0072] The drying can be carried out by conventional methods in the art. The drying time is preferably 8-24 hours, such as 10 hours or 16 hours; the drying temperature is preferably 80-150°C, such as 100°C or 120°C.
[0073] In step S3, in the post-treatment, the calcination preferably includes molding, wherein the molding can be performed by conventional methods in the art, preferably tableting, for example, tableting into cylindrical tablets.
[0074] The present invention provides a copper-zinc-magnesium-aluminum catalyst precursor, which is prepared by the preparation method of the copper-zinc-magnesium-aluminum catalyst precursor as described above.
[0075] The present invention provides a copper-zinc-magnesium-aluminum catalyst, which is obtained by reducing the copper-zinc-magnesium-aluminum catalyst precursor as described above; it comprises component A and component B'; the composition of component A is expressed as ZnO-Al2O3; the composition of component B' is expressed as Cu-MgO-Al2O3; and component A exists in a zinc-aluminum spinel structure.
[0076] Preferably, the component A is distributed in the component B'. Herein, "the component A is distributed in the component B'" means that the component A is dispersed in the component B', and may also mean that the component A is the core and the component B' is the shell, but it is not limited thereto.
[0077] In the present invention, the reduction temperature is preferably 160-260°C, for example, 170°C, 210°C or 230°C.
[0078] In the present invention, the reduction time is preferably 1-72 hours, for example 4 hours or 8 hours.
[0079] In the present invention, the reducing atmosphere may be hydrogen or a mixture of hydrogen and an inert atmosphere. The inert atmosphere may be nitrogen or an inert gas (such as argon). The inert atmosphere in the present invention refers to a gas environment that does not chemically react with the raw materials or other substances in the reaction, and is not equivalent to an inert gas.
[0080] In some embodiments of the present invention, the reducing atmosphere is a mixed gas of hydrogen and an inert atmosphere; wherein the volume proportion of the hydrogen is preferably 0.5%-20%, for example, 5% or 10%.
[0081] The present invention also provides a reaction for preparing 2,6,8-trimethyl-4-nonanone, which uses the copper-zinc-magnesium-aluminum catalyst as described above; the reaction raw materials of the reaction include methyl isobutyl carbinol; the reaction pressure is 0-2MPa; and the reaction temperature is 160-260°C.
[0082] In the present invention, the content of methyl isobutyl carbinol in the raw materials of the reaction is preferably 30%-100%, for example 50%, 60% or 70%, where the percentage is the percentage of the mass of methyl isobutyl carbinol to the total mass of the raw materials of the reaction.
[0083] Preferably, the raw materials of the reaction also include methyl isobutyl ketone; wherein the content of the methyl isobutyl ketone is preferably 20%-50%, for example 30%, 35% or 48%, where the percentage is the percentage of the mass of the methyl isobutyl ketone to the total mass of the raw materials of the reaction.
[0084] In the present invention, the raw materials of the reaction may also include impurities. The "impurities" described in the present invention refer to substances in the raw materials that do not participate in the generation of 2,6,8-trimethyl-4-nonanone. The impurities generally include one or more of C3-C9 alkanes, C3-C9 alkenes and amine compounds with benzene rings, such as 1,2,4-trimethylcyclohexane and / or aniline. Among them, "substances that do not participate in the generation of 2,6,8-trimethyl-4-nonanone" do not include methyl isobutyl carbinol or methyl isobutyl ketone that has not reacted completely.
[0085] The content of the impurities is preferably 2%-20%, for example 5% or 10%, where the percentage is the mass of the impurities relative to the total mass of the raw materials for the reaction.
[0086] In the present invention, the raw material of the reaction can be waste liquid produced by the production of rubber antioxidant 6PPD. The waste liquid produced by the production of rubber antioxidant 6PPD generally includes methyl isobutyl carbinol, methyl isobutyl ketone and the aforementioned impurities.
[0087] In a specific embodiment, the rubber antioxidant 6PPD production waste liquid includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane; wherein the content of the methyl isobutyl carbinol is 70%, the content of the methyl isobutyl ketone is 20%, and the content of the 1,2,4-trimethylcyclohexane is 10%.
[0088] In a specific embodiment, the rubber antioxidant 6PPD production waste liquid includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane; wherein the content of the methyl isobutyl carbinol is 50%, the content of the methyl isobutyl ketone is 48%, and the content of the 1,2,4-trimethylcyclohexane is 2%.
[0089] In a specific embodiment, the rubber antioxidant 6PPD production waste liquid includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane; wherein the content of the methyl isobutyl carbinol is 60%, the content of the methyl isobutyl ketone is 35%, and the content of the 1,2,4-trimethylcyclohexane is 5%.
[0090] In a specific embodiment, the rubber antioxidant 6PPD production waste liquid includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane; wherein the content of the methyl isobutyl carbinol is 60%, the content of the methyl isobutyl ketone is 30%, and the content of the 1,2,4-trimethylcyclohexane is 10%.
[0091] In the present invention, for the copper-zinc-magnesium-aluminum catalyst prepared by the present invention, a suitable reaction temperature is crucial. The present invention controls the reaction temperature within the above range, which is beneficial to improving the conversion rate of methyl isobutyl carbinol and ensuring the activity of the copper-zinc-magnesium-aluminum catalyst under long-term operation; it can also reduce the generation of side reactions and ensure the selectivity of 2,6,8-trimethyl-4-nonanone. The reaction temperature is preferably 170-260°C, for example 210°C.
[0092] For the dehydrogenation catalyst prepared by the present invention, a suitable reaction pressure is also crucial. The present invention ensures a higher conversion rate of methyl isobutyl carbinol by controlling the reaction pressure within the above range. The reaction pressure is preferably 0.1-2MPa, for example 0.2MPa. Generally speaking, normal pressure corresponds to 0MPa.
[0093] In the present invention, the liquid hourly space velocity of the reaction is preferably 0.2-2h -1 , for example 0.8h -1 or 1h -1 .
[0094] In some optional embodiments, the reaction comprises the following steps: vaporizing the raw materials of the reaction, and then introducing them into a reactor loaded with the copper-zinc-magnesium-aluminum catalyst for reaction, and obtaining the product after condensation.
[0095] In the above embodiment, the reactor is preferably a fixed bed reactor; the fixed bed reactor is, for example, a shell-and-tube fixed bed reactor, an axial adiabatic fixed bed reactor, and a radial adiabatic fixed bed reactor.
[0096] The present invention also provides the use of the copper-zinc-magnesium-aluminum catalyst in the reaction of preparing 2,6,8-trimethyl-4-nonanone; wherein the raw materials of the reaction include methyl isobutyl carbinol; the pressure of the reaction is 0-2MPa; and the temperature of the reaction is 160-260°C.
[0097] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0098] The reagents and raw materials used in the present invention are commercially available.
[0099] The positive and progressive effects of the present invention are:
[0100] The copper-zinc-magnesium-aluminum catalyst precursor of the present invention can be reduced to obtain a copper-zinc-magnesium-aluminum catalyst, and the copper-zinc-magnesium-aluminum catalyst is used in the reaction of preparing 2,6,8-trimethyl-4-nonanone, and the conversion rate of the obtained methyl isobutyl carbinol is high and the selectivity of 2,6,8-trimethyl-4-nonanone is also high. Even if the waste liquid produced by the rubber antioxidant 6PPD is used as a raw material, in the presence of impurities (such as 1,2,4-trimethylcyclohexane), the selectivity of 2,6,8-trimethyl-4-nonanone can still reach more than 90%, even more than 99%, and the conversion rate of methyl isobutyl carbinol can still reach more than 96%, even more than 99%.
[0101] By adopting the copper-zinc-magnesium-aluminum catalyst of the present invention to prepare 2,6,8-trimethyl-4-nonanone using the waste liquid produced by the rubber antioxidant 6PPD as a raw material, the utilization rate of the waste liquid produced by the rubber antioxidant 6PPD can be improved and the industrialization promotion is easy. BRIEF DESCRIPTION OF THE DRAWINGS
[0102] Figure 1 This is the GC-MS spectrum of 2,6,8-trimethyl-4-nonanone standard.
[0103] Figure 2 This is the GC-MS spectrum of 2,6,8-trimethyl-4-nonanone obtained in Example 1 of the present invention.
[0104] Figure 3 This is the XRD spectrum of the zinc-aluminum spinel structure obtained by the first precipitation reaction in Example 1 of the present invention. DETAILED DESCRIPTION
[0105] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0106] GC-MS (Model: Agilent 7890)
[0107] X-ray diffractometer (model: BRUKER D8 ADVANCE)
[0108] 2,6,8-Trimethyl-4-nonanone (CAS: 123-18-2)
[0109] Copper nitrate trihydrate (CAS: 10031-43-3)
[0110] Zinc nitrate hexahydrate (CAS: 10196-18-6)
[0111] Magnesium nitrate hexahydrate (CAS: 13446-18-9)
[0112] Aluminum nitrate nonahydrate (CAS: 7784-27-2)
[0113] Potassium hydroxide (CAS: 1310-58-3)
[0114] Potassium carbonate (CAS: 584-08-7)
[0115] Sodium hydroxide (CAS: 1310-73-2)
[0116] Sodium carbonate (CAS: 497-19-8)
[0117] Among them, the GC-MS spectrum of 2,6,8-trimethyl-4-nonanone standard is as follows Figure 1 shown.
[0118] Example 1
[0119] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0120] S1. Weigh 50g of zinc nitrate hexahydrate and 125g of aluminum nitrate nonahydrate and place them in a beaker. Add 500g of deionized water to completely dissolve them to obtain a metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L), which is recorded as solution A. Weigh 80g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction of 16%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C. Solution C is a suspension, in which the solid components in the suspension are roasted using an X-ray diffractometer and then tested by XRD. The XRD spectrum is shown as follows: Figure 3 As shown, the 2θ values corresponding to the peak positions are 18.997°, 31.265°, 36.833°, 44.791°, 49.062°, 55.629°, 59.319°, 65.197°, 74.074° and 77.291°, and the solid component has a zinc-aluminum spinel structure after calcination.
[0121] S2. Weigh 40g of copper nitrate trihydrate, 127g of magnesium nitrate hexahydrate and 125g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1 hour, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0122] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0123] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0124] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 5%) to obtain a copper-zinc-magnesium-aluminum catalyst. The reduction temperature was 210° C. and the reduction time was 4 h.
[0125] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, which is vaporized and then introduced into a fixed bed reactor for reaction. After condensation, 2,6,8-trimethyl-4-nonanone is obtained. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane, and the contents thereof are 70%, 20% and 10% respectively. The reaction temperature is 170°C, the reaction pressure is normal pressure (0 MPa), and the raw material mass liquid hourly space velocity is 1 h -1 The obtained 2,6,8-trimethyl-4-nonanone was subjected to GC-MS test using a GC-MS coupling instrument, and the obtained GC-MS spectrum is shown in Figure 2 .
[0126] Example 2
[0127] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0128] S1. Weigh 38g of zinc nitrate hexahydrate and 96g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.80mol / L), which is recorded as solution A. Weigh 60g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 12%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 40°C, and the pH is maintained at 7.5. After the precipitation is completed, maintain 40°C for aging for 1 hour, which is recorded as solution C.
[0129] S2. Weigh 36g of copper nitrate trihydrate, 159g of magnesium nitrate hexahydrate and 96g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution ((the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 112g of potassium hydroxide and 18g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction 13%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 0.5h, and the second precipitation reaction is carried out at a temperature of 40°C, maintaining the pH at 8.5.
[0130] S3, heating to 75°C for aging for 4 hours, after aging, filtering and washing the slurry. Drying the obtained solid material at 120°C for 10 hours, calcining it in a calcining furnace at 450°C for 4 hours, and finally tableting it to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0131] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0132] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 5%) to obtain a copper-zinc-magnesium-aluminum catalyst. The reduction temperature was 230° C. and the reduction time was 1 h.
[0133] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, which is vaporized and then introduced into a fixed bed reactor for reaction. After condensation, 2,6,8-trimethyl-4-nonanone is obtained. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane, with contents of 50%, 48% and 2% respectively. The reaction temperature is 170°C, the reaction pressure is 0.2 MPa, and the raw material mass liquid hourly space velocity is 1h -1 .
[0134] Example 3
[0135] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0136] S1. Weigh 32g zinc nitrate hexahydrate and 80g aluminum nitrate nonahydrate into a beaker, add 500g deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.65mol / L), which is recorded as solution A. Weigh 50g sodium carbonate, add 500g deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 50°C, and the pH is maintained at 6.5. After the precipitation is completed, maintain 50°C for aging for 0.5 hours, which is recorded as solution C.
[0137] S2. Weigh 58g of copper nitrate trihydrate, 127g of magnesium nitrate hexahydrate and 82g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 56g of sodium hydroxide and 75g of sodium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction 13.1%) is recorded as solution 2. Solution 2 is dripped into solution 1 for 1 hour, and a second precipitation reaction is carried out at a temperature of 50°C, maintaining the pH at 9.5.
[0138] S3, maintain aging at 50°C for 1 hour, filter and wash the slurry after aging. Dry the obtained solid material at 100°C for 16 hours, then roast it in a roasting furnace at 350°C for 4 hours, and finally press it into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0139] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0140] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 10%) to obtain a copper-zinc-magnesium-aluminum catalyst at a reduction temperature of 230° C. and a reduction time of 1 h.
[0141] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, which is vaporized and then introduced into a fixed bed reactor for reaction. After condensation, 2,6,8-trimethyl-4-nonanone is obtained. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane, with contents of 60%, 35% and 5% respectively. The reaction temperature is 210°C, the reaction pressure is 0.1 MPa, and the raw material mass liquid hourly space velocity is 0.8 h -1 .
[0142] Example 4
[0143] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0144] S1. Weigh 35g of zinc nitrate hexahydrate and 88g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.71mol / L), which is recorded as solution A. Weigh 50g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 40°C, and the pH is maintained at 7. After the precipitation is completed, maintain 40°C for aging for 1 hour, which is recorded as solution C.
[0145] S2. Weigh 24g of copper nitrate trihydrate, 190g of magnesium nitrate hexahydrate and 88g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 1.1 mol / L) recorded as solution 1. Weigh 300g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction 30%) is recorded as solution 2. Add solution 2 and solution 1 dropwise into solution C at the same time, the dropping time is 1h, and the second precipitation reaction is carried out at a temperature of 40°C, and the pH is maintained at 10.
[0146] S3, maintaining aging at 40°C for 2 hours, after which the aging is completed, filtering and washing the slurry. The obtained solid material is dried at 100°C for 16 hours, then roasted in a roasting furnace at 400°C for 2 hours, and finally pressed into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0147] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0148] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 5%) to obtain a copper-zinc-magnesium-aluminum catalyst at a reduction temperature of 170° C. and a reduction time of 8 h.
[0149] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, which is vaporized and then introduced into a fixed bed reactor for reaction. After condensation, 2,6,8-trimethyl-4-nonanone is obtained. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone and 1,2,4-trimethylcyclohexane, and the contents thereof are 60%, 30% and 10% respectively. The reaction temperature is 170°C, the reaction pressure is 0.1 MPa, and the raw material mass liquid hourly space velocity is 1h -1 .
[0150] Example 5
[0151] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0152] S1. Weigh 25g of zinc nitrate hexahydrate and 63g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.50mol / L), which is recorded as solution A. Weigh 50g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0153] S2. Weigh 20g of copper nitrate trihydrate, 222g of magnesium nitrate hexahydrate and 63g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1.1 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Add solution 2 and solution 1 dropwise into solution C at the same time, the dropping time is 1h, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0154] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0155] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0156] The conditions for preparing 2,6,8-trimethyl-4-nonanone are the same as those in Example 1.
[0157] Example 6
[0158] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0159] S1. Weigh 36g of zinc nitrate hexahydrate and 92g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.74mol / L), which is recorded as solution A. Weigh 50g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0160] S2. Weigh 76g of copper nitrate trihydrate, 80g of magnesium nitrate hexahydrate and 92g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 0.90 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1 hour, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0161] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0162] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0163] The conditions for preparing 2,6,8-trimethyl-4-nonanone were the same as those in Example 1.
[0164] Example 7
[0165] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0166] S1. Weigh 53g of zinc nitrate hexahydrate and 110g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.94mol / L), which is recorded as solution A. Weigh 80g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 16%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0167] S2. Weigh 28g of copper nitrate trihydrate, 102g of magnesium nitrate hexahydrate and 184g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Add solution 2 and solution 1 dropwise into solution C at the same time, the dropping time is 1h, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0168] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0169] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0170] The conditions for preparing 2,6,8-trimethyl-4-nonanone are the same as those in Example 1.
[0171] Example 8
[0172] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0173] S1. Weigh 32g zinc nitrate hexahydrate and 50g aluminum nitrate nonahydrate into a beaker, add 400g deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.60mol / L), which is recorded as solution A. Weigh 50g sodium carbonate, add 500g deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0174] S2. Weigh 73g of copper nitrate trihydrate, 123g of magnesium nitrate hexahydrate and 50g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 0.90 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1 hour, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0175] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0176] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0177] The conditions for preparing 2,6,8-trimethyl-4-nonanone are the same as those in Example 1.
[0178] Example 9
[0179] The pressure of the reaction for preparing 2,6,8-trimethyl-4-nonanone was controlled to be 2 MPa, and the other conditions were the same as those in Example 1.
[0180] Example 10
[0181] The reaction temperature for preparing 2,6,8-trimethyl-4-nonanone was controlled to be 260° C., and the other conditions were the same as those in Example 1.
[0182] Comparative Example 1
[0183] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor by one-step method
[0184] (1) Weigh 40g of copper nitrate trihydrate, 127g of magnesium nitrate hexahydrate, 50g of zinc nitrate hexahydrate and 250g of aluminum nitrate nonahydrate into a beaker, add 1500g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution A. Weigh 190g of sodium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction 19%) is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The precipitation reaction is carried out at a temperature of 70°C and the pH is maintained at 7.
[0185] (2) After precipitation, the slurry was aged at 70°C for 1 hour. After aging, the slurry was filtered and washed. The obtained solid material was dried at 80°C for 24 hours, and then calcined in a calcining furnace at 400°C for 2 hours. Finally, the copper-zinc-magnesium-aluminum catalyst precursor was obtained by tableting.
[0186] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0187] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 5%) to obtain a copper-zinc-magnesium-aluminum catalyst. The reduction temperature was 210° C. and the reduction time was 4 h.
[0188] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, vaporized, and then introduced into a fixed bed reactor for reaction, and condensed to obtain 2,6,8-trimethyl-4-nonanone. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone, and 1,2,4-trimethylcyclohexane, with mass percentages of 70%, 20%, and 10%, respectively. The reaction temperature is 170°C, the reaction pressure is normal pressure, and the raw material mass liquid hourly space velocity is 1h -1 .
[0189] Comparative Example 2
[0190] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0191] S1. Weigh 40g of copper nitrate trihydrate and 125g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L), which is recorded as solution A. Weigh 80g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 16%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0192] S2. Weigh 50g of zinc nitrate hexahydrate, 127g of magnesium nitrate hexahydrate and 125g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1 hour, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0193] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0194] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0195] (1) Preparation of copper-zinc-magnesium-aluminum catalyst: The copper-zinc-magnesium-aluminum catalyst precursor was loaded into a fixed bed reactor and reduced with a mixture of hydrogen and nitrogen (the volume fraction of hydrogen was 5%) to obtain a copper-zinc-magnesium-aluminum catalyst. The reduction temperature was 210° C. and the reduction time was 4 h.
[0196] (2) The waste liquid produced by the rubber antioxidant 6PPD is used as raw material, vaporized, and then introduced into a fixed bed reactor for reaction, and condensed to obtain 2,6,8-trimethyl-4-nonanone. The waste liquid produced by the rubber antioxidant 6PPD includes methyl isobutyl carbinol, methyl isobutyl ketone, and 1,2,4-trimethylcyclohexane, with mass percentages of 70%, 20%, and 10%, respectively. The reaction temperature is 170°C, the reaction pressure is normal pressure, and the raw material mass liquid hourly space velocity is 1h -1 .
[0197] Comparative Example 3
[0198] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0199] S1. Weigh 15g of zinc nitrate hexahydrate and 94g of aluminum nitrate nonahydrate into a beaker, add 500g of deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.60mol / L), which is recorded as solution A. Weigh 50g of sodium carbonate, add 500g of deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0200] S2. Weigh 94g of copper nitrate trihydrate, 67g of magnesium nitrate hexahydrate and 63g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 0.80mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1h, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0201] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0202] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0203] The conditions for preparing 2,6,8-trimethyl-4-nonanone are the same as those in Example 1.
[0204] Comparative Example 4
[0205] 1. Preparation of copper-zinc-magnesium-aluminum catalyst precursor
[0206] S1. Weigh 149g zinc nitrate hexahydrate and 125g aluminum nitrate nonahydrate into a beaker, add 1000g deionized water to completely dissolve them, and obtain a metal salt aqueous solution (the molar concentration of the metal salt is 0.80mol / L), which is recorded as solution A. Weigh 106g sodium carbonate, add 1060g deionized water and stir evenly to form a precipitant solution (mass fraction is 10%), which is recorded as solution B. Under stirring conditions, solution A and solution B are added to the reactor at the same time. The first precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 7. After the precipitation is completed, maintain 70°C for aging for 1 hour, which is recorded as solution C.
[0207] S2. Weigh 40g of copper nitrate trihydrate, 127g of magnesium nitrate hexahydrate and 125g of aluminum nitrate nonahydrate into a beaker, add 1000g of deionized water to completely dissolve them, and the resulting metal salt aqueous solution (the molar concentration of the metal salt is 1 mol / L) is recorded as solution 1. Weigh 80g of potassium hydroxide and 100g of potassium carbonate, add 1000g of deionized water and stir evenly, and the resulting precipitant solution (mass fraction is 18%) is recorded as solution 2. Solution 2 and solution 1 are simultaneously dripped into solution C for 1 hour, and the second precipitation reaction is carried out at a temperature of 70°C, and the pH is maintained at 9.
[0208] S3, after precipitation, continue aging at 70°C for 2 hours, filter and wash the slurry after aging, dry the obtained solid material at 80°C for 24 hours, calcine in a calcining furnace at 400°C for 2 hours, and finally press into tablets to obtain a copper-zinc-magnesium-aluminum catalyst precursor.
[0209] 2. Preparation of 2,6,8-trimethyl-4-nonanone
[0210] The conditions for preparing 2,6,8-trimethyl-4-nonanone were the same as those in Example 1.
[0211] Comparative Example 5
[0212] The temperature of the first precipitation reaction in step S1 and the second precipitation reaction in step S2 were controlled to be 90° C., and the other conditions were kept consistent with those in Example 1.
[0213] Comparative Example 6
[0214] The endpoint pH value of the second precipitation reaction in step S2 is controlled to be 7, and the other conditions are consistent with those in Example 1.
[0215] Comparative Example 7
[0216] The calcination temperature in step S3 is controlled to be 600° C., and the other conditions are consistent with those in Example 1.
[0217] Comparative Example 8
[0218] The pressure of the reaction for preparing 2,6,8-trimethyl-4-nonanone was controlled to be 4 MPa, and the other conditions were the same as those in Example 1.
[0219] Comparative Example 9
[0220] The reaction temperature for preparing 2,6,8-trimethyl-4-nonanone was controlled to be 350° C., and the other conditions were the same as those in Example 1.
[0221] The measured element molar ratios and oxide contents of the copper-zinc-magnesium-aluminum catalyst precursors prepared in the above Examples 1-10 and Comparative Examples 1-9 are shown in Tables 1 and 2.
[0222] Table 1
[0223]
[0224]
[0225] Table 2
[0226]
[0227]
[0228] The specific reaction conditions and results for preparing 2,6,8-trimethyl-4-nonanone in the above Examples 1-10 and Comparative Examples 1-9 are shown in Table 3, where:
[0229] (1) The calculation formula of methyl isobutyl carbinol conversion rate is:
[0230]
[0231] Where:
[0232] ω1: the mass fraction of methyl isobutyl carbinol in the raw material, expressed in %;
[0233] ω2: The mass fraction of methyl isobutyl carbinol in the product, expressed in %.
[0234] (2) The calculation formula for the selectivity of 2,6,8-trimethyl-4-nonanone is:
[0235]
[0236] Where:
[0237] n1: the value of the mole fraction of methyl isobutyl carbinol in the raw material, expressed in %;
[0238] n2: the value of the mole fraction of methyl isobutyl carbinol in the product, expressed in %;
[0239] n3: The numerical value of the molar fraction of 2,6,8-trimethyl-4-nonanone in the product, expressed in %.
[0240] Table 3
[0241]
[0242]
[0243] From Table 1, Table 2 and Table 3, we can see that:
[0244] From the comparison of the methyl isobutyl carbinol conversion rate and the 2,6,8-trimethyl-4-nonanone selectivity of Example 1-10 and Comparative Example 1-9, it can be seen that Example 1-10 of the present invention uses a copper-zinc-magnesium-aluminum catalyst as a catalyst and adopts the rubber antioxidant 6PPD production waste liquid as a raw material to prepare 2,6,8-trimethyl-4-nonanone, which can take into account a higher methyl isobutyl carbinol conversion rate and a higher 2,6,8-trimethyl-4-nonanone selectivity. Specifically, the methyl isobutyl carbinol conversion rate can reach more than 96%, or even more than 99%, and the 2,6,8-trimethyl-4-nonanone selectivity can reach more than 90%, or even more than 99%.
[0245] Compared with Example 1 using the two-step precipitation method, the difference of Comparative Example 1 is only that the copper-zinc-magnesium-aluminum catalyst precursor is prepared by the one-step precipitation method, and the obtained methyl isobutyl carbinol conversion rate and 2,6,8-trimethyl-4-nonanone selectivity are greatly reduced. This may be because the two-step method is used to first prepare a stable zinc-aluminum spinel structure, thereby effectively isolating the active components, which not only improves the catalyst's ability to resist impurities, but also helps to improve the high-temperature stability of the catalyst, while the one-step method cannot achieve the above purpose.
[0246] In Example 1, the first precipitation reaction generates zinc-aluminum spinel, and then copper-magnesium-aluminum is co-precipitated through the second precipitation reaction. In Comparative Example 2, the first precipitation reaction generates copper-aluminum precipitate, and then zinc-magnesium-aluminum is co-precipitated through the second precipitation reaction to prepare a copper-zinc-magnesium-aluminum catalyst precursor. The obtained methyl isobutyl carbinol conversion rate and 2,6,8-trimethyl-4-nonanone selectivity are greatly reduced. This may be because the active components in the copper-zinc-magnesium-aluminum catalyst obtained in Comparative Example 2 cannot effectively contact the reaction raw materials, thereby failing to effectively exert a catalytic effect.
[0247] From the comparison between Comparative Example 3 and Example 1, it can be seen that the molar ratio of Cu and Mg in component B of the catalyst precursor of Comparative Example 3 is 1.49:1, which is too large, and the conversion rate of methyl isobutyl carbinol and the selectivity of 2,6,8-trimethyl-4-nonanone obtained are reduced. This may be because Cu is an active component in the catalyst. When the molar ratio of Cu and Mg in component B is too large, the Cu crystals in the obtained catalyst are too large, and the relative specific surface area is reduced, resulting in a reduction in the actual catalytic active sites, thereby reducing the catalytic activity or even deactivating it.
[0248] From the comparison between Comparative Example 4 and Example 1, it can be seen that the molar ratio of Zn and Al elements in component A of the catalyst precursor of Comparative Example 4 is 1.5:1. If the molar ratio is too large, the conversion rate of methyl isobutyl carbinol and the selectivity of 2,6,8-trimethyl-4-nonanone are further reduced. This may be because the spinel structure can only be formed when the molar ratio of Zn and Al elements in component A is within an appropriate range, but not if it is too large.
[0249] By comparing Comparative Example 5 with Example 1, it can be seen that the temperature of the first precipitation reaction in step S1 of Comparative Example 5 and the second precipitation reaction in step S2 are both 90°C, which is too high. The conversion rate of the obtained methyl isobutyl carbinol is reduced, and the selectivity of 2,6,8-trimethyl-4-nonanone is significantly reduced. This may be because the temperature of the first precipitation reaction is too high to form a spinel structure, and the temperature of the second precipitation reaction is too high, which will also destroy the formation of the catalyst precursor, thereby reducing the catalytic performance of the obtained copper-zinc-magnesium-aluminum catalyst.
[0250] By comparing Comparative Example 6 with Example 1, it can be seen that the pH value of the second precipitation reaction in step S2 of Comparative Example 6 is 7, which is too small, and the conversion rate of methyl isobutyl carbinol and the selectivity of 2,6,8-trimethyl-4-nonanone obtained are greatly reduced. This is because the endpoint pH value of the precipitation reaction is a key factor in the synthesis process of the copper-zinc-magnesium-aluminum catalyst precursor. The endpoint pH value of the precipitation reaction determines the structure and surface properties of the copper-zinc-magnesium-aluminum catalyst precursor, and thus also has a significant effect on the structure and performance of the copper-zinc-magnesium-aluminum catalyst obtained by reduction. In the present invention, the endpoint pH value of the second precipitation reaction is 8-11, which is alkaline, which is conducive to neutralizing the acid sites of the obtained copper-zinc-magnesium-aluminum catalyst precursor, and then reducing the acid sites of the obtained copper-zinc-magnesium-aluminum catalyst, thereby achieving the purpose of reducing side reactions and improving the selectivity of 2,6,8-trimethyl-4-nonanone.
[0251] In addition, when the endpoint pH value of the first precipitation reaction is less than 6, the zinc-aluminum spinel structure cannot be formed. When the endpoint pH value of the first precipitation reaction is greater than 8, the zinc-aluminum spinel structure cannot be formed. Therefore, when the endpoint pH value of the first precipitation reaction is too large or too small, the obtained catalyst is used to prepare 2,6,8-trimethyl-4-nonanone, and it is impossible to take into account both a high methyl isobutyl carbinol conversion rate and a high 2,6,8-trimethyl-4-nonanone selectivity.
[0252] Compared with Example 1, the calcination temperature in step S3 of Comparative Example 7 is 600° C., which is too high, and the conversion rate of the obtained methyl isobutyl carbinol is reduced, while the selectivity of 2,6,8-trimethyl-4-nonanone is significantly reduced.
[0253] Compared with Example 1, the pressure of the reaction for preparing 2,6,8-trimethyl-4-nonanone in Comparative Example 8 is 4 MPa, which is too large. Although the conversion rate of the obtained methyl isobutyl carbinol is high, the selectivity of 2,6,8-trimethyl-4-nonanone is significantly reduced. This is because the reaction of using rubber antioxidant 6PPD production waste liquid as a raw material to generate 2,6,8-trimethyl-4-nonanone is a reaction in which the volume increases, which makes the reaction pressure higher, thereby inhibiting the reaction, which is not conducive to the generation of 2,6,8-trimethyl-4-nonanone.
[0254] By comparing Comparative Example 9 with Example 1, it can be seen that the reaction temperature for preparing 2,6,8-trimethyl-4-nonanone in Comparative Example 9 is 350° C., which is too high. Although the conversion rate of the obtained methyl isobutyl methanol is high, the selectivity of 2,6,8-trimethyl-4-nonanone is significantly reduced. This is because the high reaction temperature will reduce the catalytic activity of the catalyst, resulting in more by-products, thereby causing the selectivity of 2,6,8-trimethyl-4-nonanone to be significantly reduced.
[0255] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A copper-zinc-magnesium-aluminum catalyst precursor, It is characterized in that It includes component A and component B; the composition of component A is expressed as ZnO-Al 2 O 3 ; The composition of component B is expressed as CuO-MgO-Al 2 O 3 ;in, The component A exists in a zinc-aluminum spinel structure; In the component A, the molar ratio of Zn to Al is (0.10-1):1; In the component B, the molar ratio of Cu and Mg elements is (0.10-1.01):
1.
2. The copper-zinc-magnesium-aluminum catalyst precursor according to claim 1, It is characterized in that It satisfies one or more of the following conditions: a. In the component A, the molar ratio of Zn to Al is (0.30-1):1, for example, 0.49:1, 0.50:1, 0.61:1 or 0.81:1; b. In the component B, the molar ratio of Cu and Mg is (0.10-0.80):1, preferably (0.10-0.50):1; in the component B, the molar ratio of Cu and Mg is, for example, 0.13:1, 0.24:1, 0.29:1, 0.33:1, 0.48:1 or 0.63:1; c. In the component B, the molar ratio of the sum of the molar numbers of the Cu and Mg elements to the Al element is (0.50-6):1, preferably (1-5):1; in the component B, the molar ratio of the sum of the molar numbers of the Cu and Mg elements to the Al element is, for example, 1.05:1, 1.98:1, 2.55:1, 3.01:1, 3.36:1 or 3.58:1, 5.65:1 or 5.87:1; d. The molar ratio of Al element in the component A to that in the component B is (0.60-2):1, for example, 0.98:1 or 1:1; e. In the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Cu to Al elements is (0.14-1.14):1, for example, 0.15:1, 0.21:1, 0.25:1, 0.29:1, 0.56:1, 0.64:1 or 1.13:1; f. In the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Zn to Al is (0.23-0.40):1, for example, 0.25:1; g. In the copper-zinc-magnesium-aluminum catalyst precursor, the molar ratio of Mg to Al is (0.51-2.58):1, for example, 0.64:1, 0.74:1, 1.15:1, 1.21:1, 1.58:1 or 1.80:1; h. In the copper-zinc-magnesium-aluminum catalyst precursor, the content of CuO is 10%-40%, for example, 10.1%, 11.1%, 11.6%, 16.2%, 16.3%, 16.7%, 27.3%, 34.5% or 36.6%, where the percentage is the mass percentage of CuO in the copper-zinc-magnesium-aluminum catalyst precursor; i. In the copper-zinc-magnesium-aluminum catalyst precursor, the content of ZnO is 5%-20%, for example, 10.5%, 12.5%, 13.3%, 13.4%, 13.6%, 14.2%, 16.9% or 18.2%, where the percentage is the mass percentage of ZnO in the copper-zinc-magnesium-aluminum catalyst precursor; j. In the copper-zinc-magnesium-aluminum catalyst precursor, the content of MgO is 17%-60%, for example, 17.4%, 20.1%, 24.7%, 28.6%, 29.4%, 34.1%, 41.9% or 53.3%, where the percentage is the mass percentage of MgO in the copper-zinc-magnesium-aluminum catalyst precursor; k. In the copper-zinc-magnesium-aluminum catalyst precursor, the Al 2 O 3 The content of Al is 15%-55%, for example, 20.7%, 26.2%, 31.6%, 33.6%, 34.5%, 35.5%, 42.1% or 50.1%, and the percentage is Al 2 O 3 The mass percentage of the copper-zinc-magnesium-aluminum catalyst precursor; 1. The component A is distributed in the component B.
3. A method for preparing a copper-zinc-magnesium-aluminum catalyst precursor, It is characterized in that It adopts a two-step precipitation method, which includes the following steps: S1. Performing a first precipitation reaction on a first precipitant aqueous solution and a first metal salt aqueous solution to obtain a mixed solution; wherein the first metal salt aqueous solution comprises a zinc salt and an aluminum salt; in the first metal salt aqueous solution, the molar ratio of Zn to Al is (0.10-1):1; the temperature of the first precipitation reaction is 40-80°C; and the endpoint pH value of the first precipitation reaction is 6-8; S2, adding a second metal salt aqueous solution and a second precipitant aqueous solution to the mixed solution to carry out a second precipitation reaction; wherein the second metal salt aqueous solution comprises copper salt, magnesium salt and aluminum salt; the temperature of the second precipitation reaction is 40-80° C.; the endpoint pH value of the second precipitation reaction is 8-11; in the second metal salt aqueous solution, the molar ratio of Cu and Mg elements is (0.10-1.01):1; S3, after post-treatment, the product is obtained; wherein the post-treatment includes calcination; the calcination temperature is 300-500°C.
4. The method for preparing the copper-zinc-magnesium-aluminum catalyst precursor as claimed in claim 3, It is characterized in that It satisfies one or more of the following conditions ao: a. In step S1, the metal salt in the first metal salt aqueous solution includes one or more of nitrate, chlorate, sulfate and acetate; b. In step S2, the metal salt in the second metal salt aqueous solution includes one or more of nitrate, chlorate, sulfate and acetate; c. In step S1, the concentration of the metal salt in the first metal salt aqueous solution is 0.2-4 mol / L, for example, 0.50 mol / L, 0.60 mol / L, 0.65 mol / L, 0.71 mol / L, 0.74 mol / L, 0.80 mol / L, 0.94 mol / L or 1 mol / L; d. In step S2, the concentration of the metal salt in the second metal salt aqueous solution is 0.2-4 mol / L, for example, 0.90 mol / L, 1 mol / L or 1.1 mol / L; e. In step S1, the precipitant in the first precipitant aqueous solution is an alkaline substance, preferably comprising K 2 CO 3 、Na 2 CO 3 , NaOH, NaHCO 3 and KOH; f. In step S2, the precipitant in the second precipitant aqueous solution is an alkaline substance, preferably comprising K 2 CO 3 、Na 2 CO 3 , NaOH, NaHCO 3 and KOH; g. In step S1, the mass fraction of the precipitant in the first precipitant aqueous solution is 5%-30%, for example, 10%, 12% or 16%; h. In step S2, the mass fraction of the precipitant in the second precipitant aqueous solution is 5%-30%, for example, 13%, 13.1% or 18%; i. In step S2, in the second aqueous metal salt solution, the molar ratio of the sum of the molar numbers of Cu and Mg elements to the Al element is (0.50-6):1; preferably (1-5):1; in the component B, the molar ratio of the sum of the molar numbers of Cu and Mg elements to the Al element is, for example, 1.05:1, 1.98:1, 2.55:1, 3.01:1, 3.36:1, 3.58:1, 5.65:1 or 5.87:1; j. In step S1 and step S2, the molar ratio of Al element in the first metal salt aqueous solution and the second metal salt aqueous solution is (0.60-2):1, for example, 0.98:1 or 1:1; k. In step S1, after the first precipitation reaction is completed, an aging step is further included; the aging temperature is preferably 40-70° C., for example, 50° C.; the aging time is preferably 0.5-1 h; 1. In step S3, the calcination temperature is 350-450° C., for example, 400° C.; m. In step S3, the calcination time is 0.5-4h, for example, 2h; n. In step S3, in the post-treatment, the calcination further includes aging, washing, filtering and drying; wherein the aging time is preferably 0.5-6h, for example, 1h, 2h or 4h; the aging temperature is preferably 40-80°C, for example, 50°C, 70°C or 75°C; the washing detergent is preferably deionized water; the drying time is preferably 8-24h, for example, 10h or 16h; the drying temperature is preferably 80-150°C, for example, 100°C or 120°C; o. In step S3, in the post-processing, the calcination further includes molding; wherein the molding is preferably tableting.
5. A copper-zinc-magnesium-aluminum catalyst precursor, It is characterized in that The catalyst is prepared by the method for preparing the copper-zinc-magnesium-aluminum catalyst precursor according to claim 3 or 4.
6. A copper-zinc-magnesium-aluminum catalyst, It is characterized in that It is obtained by reducing the copper-zinc-magnesium-aluminum catalyst precursor according to any one of claims 1-2 and 5; the copper-zinc-magnesium-aluminum catalyst comprises component A and component B'; the composition of component A is expressed as ZnO-Al 2 O 3 ; The composition of component B' is expressed as Cu-MgO-Al 2 O 3 ; The component A exists in a zinc-aluminum spinel structure.
7. The copper-zinc-magnesium-aluminum catalyst according to claim 6, It is characterized in that The reduction satisfies one or more of the following conditions ac: a. The reduction temperature is 160-260°C, for example, 170°C, 210°C or 230°C; b. The reduction time is 1-72 hours, for example 4 hours or 8 hours; c. The reducing atmosphere is hydrogen or a mixture of hydrogen and an inert atmosphere; wherein, in the mixture of hydrogen and an inert atmosphere, the volume proportion of hydrogen is preferably 0.5%-20%, for example, 5% or 10%.
8. A reaction for preparing 2,6,8-trimethyl-4-nonanone, which uses the copper-zinc-magnesium-aluminum catalyst as described in claim 6 or 7; the reaction raw materials of the reaction include methyl isobutyl carbinol; the reaction pressure is 0-2MPa; the reaction temperature is 160-260°C.
9. The reaction for preparing 2,6,8-trimethyl-4-nonanone as claimed in claim 8, It is characterized in that The reaction satisfies one or more of the following conditions ah: a. In the raw materials of the reaction, the content of methyl isobutyl carbinol is 30%-100%, for example, 50%, 60% or 70%, where the percentage is the percentage of the mass of methyl isobutyl carbinol to the total mass of the raw materials of the reaction; b. The raw materials of the reaction further include methyl isobutyl ketone; wherein the content of the methyl isobutyl ketone is preferably 20%-50%, for example, 30%, 35% or 48%, where the percentage is the mass of the methyl isobutyl ketone to the total mass of the raw materials of the reaction; c. The raw materials of the reaction also include impurities; The content of the impurities is preferably 2%-20%, for example 5% or 10%, where the percentage is the mass of the impurities as a percentage of the total mass of the raw materials for the reaction; the impurities preferably include C 3 -C 9 Alkanes, C 3 -C 9 One or more of olefins and amine compounds with a benzene ring, such as 1,2,4-trimethylcyclohexane and / or aniline; d. The raw material of the reaction is waste liquid from the production of rubber antioxidant 6PPD; e. The reaction temperature is 170-260° C., for example, 210° C.; f. The reaction pressure is 0.1-2 MPa, for example 0.2 MPa; g. The liquid hourly space velocity of the reaction is 0.2-2h -1 , for example 0.8h -1 or 1h -1 ; h. The reaction comprises the following steps: vaporizing the raw materials of the reaction, and then introducing them into a reactor loaded with the copper-zinc-magnesium-aluminum catalyst for reaction, and condensing to obtain the product; The reactor is preferably a fixed bed reactor, such as a tube-in-tube fixed bed reactor, an axial adiabatic fixed bed reactor and a radial adiabatic fixed bed reactor.
10. Use of the copper-zinc-magnesium-aluminum catalyst as claimed in claim 6 or 7 in the preparation of 2,6,8-trimethyl-4-nonanone, It is characterized in that The raw material of the reaction includes methyl isobutyl carbinol; the pressure of the reaction is 0-2MPa; and the temperature of the reaction is 160-260°C.
Citation Information
Patent Citations
A process for one-step synthesis of 2,6,8-trimethyl-4-nonanone from catalytic methyl isobutyl ketone.
CN107935830B
Dehydrogenation catalyst as well as precursor, preparation method and application thereof
CN117839703A
Hydrotalcite-like catalyst as well as precursor, preparation method and application thereof
CN117861663A
Process for preparing Cu-Zn-Al vapor hydroformylation catalyst and products therefrom
CN1883795A
process for preparing saturated and / or unsaturated carbonyl compounds in a single step.
NL7007461A