Catalyst for preparing carbon nano tube, preparation method and application of catalyst for preparing carbon nano tube

By using alumina and rectorite as composite carriers to load catalysts with metal components such as iron, cobalt and bismuth, the problems of high cost and insufficient growth rate in the preparation of existing carbon nanotubes are solved, and high efficiency and high purity are achieved. Carbon nanotube preparation.

CN118767929AInactive Publication Date: 2024-10-15CHANGZHOU GUOXIN MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410765717.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing carbon nanotube preparation technology has problems such as high preparation cost and insufficient growth rate. Especially in the chemical vapor deposition method, the performance of the catalyst needs to be further improved.

Method used

Alumina and rectorite are used as composite carriers, and rectorite is activated by pickling and high-temperature alkali treatment, and metal components such as iron, cobalt, and bismuth are loaded in the catalyst, and an efficient catalyst is formed through multiple impregnation and calcination treatments. for the preparation of carbon nanotubes.

Benefits of technology

It significantly improves the growth rate and purity of carbon nanotubes, improves the catalytic performance of the catalyst, and achieves efficient and cost-controllable preparation of carbon nanotubes.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing a carbon nano tube, a preparation method and application of the catalyst for preparing the carbon nano tube. The preparation method of the catalyst comprises the steps of hydrochloric acid solution cleaning, high-temperature sodium hydroxide treatment, grinding and sieving treatment, iron loading, cobalt loading, bismuth loading and the like. According to the catalyst for preparing the carbon nanotubes, the aluminum oxide and the rectorite are creatively matched to serve as a composite carrier, and efficient loading of the active components and the auxiliary active components is guaranteed; meanwhile, bismuth is widely screened as an auxiliary active component, and the performance of the catalyst is remarkably improved, so that the obtained catalyst is high in growth rate and relatively high in purity in the preparation process of the carbon nanotube, and the production cost is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon nanotube preparation, and specifically relates to a catalyst for preparing carbon nanotubes, a preparation method and application of the prepared carbon nanotubes. Background Art

[0002] Nanocarbon materials are a new type of nanomaterials, mainly including carbon nanotubes, carbon nanofibers, and carbon nanospheres. Among them, carbon nanotubes have shown broad application prospects since they were discovered in 1991, due to their unique structure and excellent mechanical, electrical and chemical properties. They have attracted great attention from many scientists in the fields of materials, physics, electronics, chemistry, etc., and have become the research frontier and hotspot in the field of international new materials.

[0003] At present, the preparation of carbon nanotubes mainly includes three methods: arc discharge method, laser ablation method and chemical vapor deposition method. The arc discharge method uses graphite rods as the positive and negative electrodes, and the anode graphite rod is loaded with catalyst particles. In a vacuum reaction chamber filled with a certain inert gas, hydrogen or other gas, the solid graphite carbon source of the anode is evaporated by the high-temperature arc generated between the two electrodes, so that the carbon atoms are precipitated into tubular, granular, etc. at the cathode; the carbon nanotubes prepared by the arc discharge method have a high degree of graphitization and fewer defects, but this method has high requirements for equipment, high growth temperature and low yield. The laser ablation method, also known as the laser evaporation method, is a method of preparing carbon nanotubes by bombarding a transition metal-doped graphite target with a laser under the protection of an inert gas at a temperature of about 1200°C to form gaseous carbon atoms under the action of a catalyst; the carbon nanotubes prepared by the laser ablation method have a high purity and controllable conditions, but the equipment used is expensive and the production cost is high. Chemical vapor deposition (CVD) is a method of decomposing a carbon source in the presence of a catalyst at a relatively low temperature, causing the carbon atoms to dissolve on the catalyst particles and precipitate in the form of tubes to form carbon nanotubes. CVD is considered one of the most promising methods due to its mild reaction conditions and high yield.

[0004] In the process of preparing carbon nanotubes by chemical vapor deposition, the use of catalysts is very important. Studies have shown that transition metals such as iron, cobalt, nickel, etc. are the preferred active metal components for the preparation of carbon nanotubes, and common carriers include aluminum oxide, magnesium oxide, silicon dioxide, graphite, etc. In the prior art, patent document CN115672345A uses magnesium aluminum hydrotalcite as a carrier and adopts a solvent thermal method to prepare a carbon nanotube catalyst; the carbon nanotube catalyst provided by patent document CN104884384B uses calcined aluminum hydroxide to form a carrier, loads main catalysts such as cobalt and iron, and is matched with a loaded auxiliary catalyst vanadium; the carbon nanotube catalyst provided by patent document CN110586115B is a nano multi-metal alloy phase, which reduces the agglomeration of metal nanoparticles, and rare earth metal lanthanum is used. In the above-mentioned prior art, the preparation of carbon nanotubes still has problems such as relatively high preparation cost and insufficient growth rate of carbon nanotubes. Developing a new catalyst with high efficiency and controllable cost is still a topic worthy of in-depth study in the preparation process of carbon nanotubes. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention aims to provide a catalyst for preparing carbon nanotubes, a preparation method and an application of preparing carbon nanotubes. The prepared carbon nanotubes have a high growth rate, high purity and good catalytic effect.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for preparing a catalyst for preparing carbon nanotubes, comprising the following steps:

[0008] (1) washing the rectorite with a hydrochloric acid solution, and then separating and washing it to a neutral state to obtain a pre-modified rectorite;

[0009] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide and subjecting the mixture to high temperature treatment, and obtaining modified rectorite after the treatment;

[0010] (3) mixing the alumina and the modified rectorite obtained in step (2), grinding and sieving the mixture to obtain a composite carrier;

[0011] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the iron loading;

[0012] (5) adding the material loaded with iron in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the loading of cobalt;

[0013] (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining to obtain a catalyst product.

[0014] As a further preferred embodiment of the technical solution of the present invention, in step (1), the concentration of the hydrochloric acid solution is 0.8 to 1.5 mol / L, and the dosage ratio of rectorite to the hydrochloric acid solution is 1 g: 5 to 15 mL.

[0015] As a further preferred embodiment of the technical solution of the present invention, in step (2), the mass ratio of the pre-modified rectorite to sodium hydroxide is 1:0.01-0.1, the high temperature treatment temperature is 790-820°C, and the treatment time is 0.5-6h.

[0016] As a further preferred embodiment of the technical solution of the present invention, in step (3), the mass ratio of alumina to modified rectorite is 1:0.3-0.6; and the sieve mesh number is 100-250 meshes.

[0017] As a further preferred embodiment of the technical solution of the present invention, in step (4), the concentration of ferric chloride is 0.1-0.25 mol / L, the mass ratio of the composite carrier, ferric chloride and water is 10:0.4-0.8:80-150; the calcination temperature is 480-550°C, and the calcination time is 0.5-6h.

[0018] As a further preferred embodiment of the technical solution of the present invention, in step (5), the concentration of the cobalt chloride solution is 0.08-0.15 mol / L; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.25-0.4:80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h.

[0019] As a further preferred embodiment of the technical solution of the present invention, in step (6), the concentration of the bismuth nitrate solution is 0.08-0.15 mol / L, the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g: 0.08-0.15: 80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h.

[0020] In a second aspect, the present invention provides a method for protecting a catalyst prepared by the above method.

[0021] In a third aspect, the present invention provides a use of the above catalyst in the preparation of carbon nanotubes.

[0022] As a further preferred embodiment of the above application, the preparation of carbon nanotubes comprises the following steps: placing the catalyst in a quartz glass tube reactor, and then introducing nitrogen for replacement;

[0023] Subsequently, the nitrogen gas is stopped and switched to a mixed gas of ethylene, hydrogen and nitrogen. The quartz glass tube reactor is heated to 620-800°C. After reacting for 0.5-6 hours, the heating and the methane gas are stopped. After cooling, carbon nanotubes are obtained.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The carbon nanotube catalyst provided by the present invention creatively uses a combination of alumina and rectorite as a composite carrier, thereby ensuring efficient loading of active components and co-active components, so that the obtained catalyst has a high growth rate and high purity during the preparation process of carbon nanotubes.

[0026] (2) In the preparation process of rectorite, the present invention performs certain modification treatment on the rectorite. Specifically, the rectorite is firstly acid-washed to remove impurities and play a role of preliminary activation; then the pre-modified rectorite is subjected to high-temperature alkali treatment to achieve the purpose of secondary activation. Through the above treatment, the active components and co-active components are fully loaded in the subsequent loading process, thereby improving the catalytic performance of the catalyst.

[0027] (3) The carbon nanotube catalyst provided by the present invention not only carries common iron and nickel active ingredients, but also widely selects bismuth as an auxiliary active component based on the macroscopic formation mechanism of carbon nanotube catalytic thermal cracking, so that the performance of the catalyst is significantly improved. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Unless otherwise specified, all commodities in the present invention are purchased through market channels. Alumina is γ-alumina with a pore volume greater than 0.21 cm 3 / g.

[0030] The present invention provides a method for preparing a catalyst for preparing carbon nanotubes, comprising the following steps:

[0031] (1) washing the rectorite with a hydrochloric acid solution, and then separating and washing it to a neutral state to obtain a pre-modified rectorite;

[0032] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide and subjecting the mixture to high temperature treatment, and obtaining modified rectorite after the treatment;

[0033] (3) mixing the alumina and the modified rectorite obtained in step (2), grinding and sieving the mixture to obtain a composite carrier;

[0034] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the iron loading;

[0035] (5) adding the material loaded with iron in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the loading of cobalt;

[0036] (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining to obtain a catalyst product.

[0037] In the above technical solution, rectorite and alumina are used as raw materials for the composite carrier. Alumina has been reported to be used in the preparation of carbon nanotube catalysts. Other commonly used carriers include silica, graphite, etc. The above rectorite carrier is the first time the applicant has creatively reported its use. The rectorite raw material may contain certain impurities and not have rich pores. Therefore, two modifications are carried out during the preparation process, one is acid washing and the other is high-temperature alkali melting, to ensure the full activation of the rectorite.

[0038] After the composite carrier is prepared, the three metal components of iron, cobalt and bismuth are loaded by multiple impregnations, and the process is simple. It should be noted that the loading of the above metal components can also be prepared by coprecipitation method, combustion method, etc., and is not completely limited to the impregnation method shown above.

[0039] In the above technical solution, the introduction of bismuth is also creatively proposed by the applicant. At present, there are different theoretical model studies on the preparation of carbon nanotubes by chemical vapor deposition, but the macroscopic processes involved all include the decomposition of carbon sources at high temperatures to produce carbon atoms. This process involves a thermal decomposition process. Based on this, the present invention has found through extensive screening that the introduction of bismuth can greatly improve the performance of the catalyst. Its action pathway may be: improving the distribution of active components iron and cobalt, thereby achieving the purpose of regulating the activity of the catalyst.

[0040] In step (1) of the catalyst preparation process, the concentration of the hydrochloric acid solution is 0.8-1.5 mol / L, and the ratio of rectorite to the hydrochloric acid solution is 1 g: 5-15 mL. It is understandable that the concentration of the hydrochloric acid solution can be optimized and adjusted, such as 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L or any value within the above range. Similarly, the ratio of rectorite to the hydrochloric acid solution can also be flexibly adjusted, such as when the amount of rectorite is 1 g, the amount of the hydrochloric acid solution can be 5 mL, 6 mL, 7 mL, 8 mL, 9 mL, 10 mL, 11 mL, 12 mL, 13 mL, 14 mL, 15 mL or any value within the above range. Preferably, the concentration of the hydrochloric acid solution is 1 mol / L, and the dosage ratio of rectorite to the hydrochloric acid solution is 1 g:10 mL.

[0041] In step (2) of the catalyst preparation process, the mass ratio of pre-modified rectorite to sodium hydroxide is 1:0.01-0.1. It is understood that the mass ratio of sodium hydroxide to pre-modified rectorite can be flexibly adjusted, such as 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05, 1:0.06, 1:0.07, 1:0.08, 1:0.09, 1:0.1 or any numerical ratio within the above range. Preferably, the mass ratio of pre-modified rectorite to sodium hydroxide is 1:0.08. The temperature of the high temperature treatment is 790-820°C, and the treatment time is 0.5-6h. The above treatment temperature and treatment time can also be adjusted within a reasonable range. For example, the treatment temperature can be 790°C, 791°C, 792°C, 793°C, 794°C, 795°C, 796°C, 797°C, 798°C, 799°C, 800°C, 801°C, 802°C, 803°C, 804°C, 805°C, 806°C, 807°C, 808°C The temperature of the heating element can be 8°C, 809°C, 810°C, 811°C, 812°C, 813°C, 814°C, 815°C, 816°C, 817°C, 818°C, 819°C, 820°C or any value within the above range; the processing time can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h or any value within the above range.

[0042] In step (3) of the preparation process of the above catalyst, the mass ratio of alumina to modified rectorite is 1:0.3-0.6; the sieve mesh is 100-250 mesh. In the present invention, the amount of alumina accounts for the majority, and a small amount of rectorite is used in combination to enrich the pore distribution and improve the loading effect of the active component. It can be understood that the mass ratio of alumina to modified rectorite can be a numerical ratio of 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6 or any numerical ratio within the above range. The sieve mesh is preferably 200 mesh.

[0043] In the steps (4), (5) and (6) of the preparation process of the above catalyst, the impregnation loading of iron, cobalt and bismuth is carried out in sequence, which is a routine operation and is subject to the ability of a person skilled in the art to implement. The use form of each metal salt is not limited to the specific examples, such as iron salts can choose common iron salt forms such as ferric chloride, ferric nitrate, ferric sulfate, and ferric acetate, cobalt salts can choose common cobalt source forms such as cobalt chloride, cobalt nitrate, and cobalt acetate, and the same is true for bismuth salts. The concentration of the above metal salts and the calcination temperature and time of the final impregnation loading are slightly different, but they are similar. Specifically, in step (4), the concentration of ferric chloride is 0.1-0.25 mol / L, the mass ratio of the composite carrier, ferric chloride and water is 10: 0.4-0.8: 80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h; in step (5), the concentration of the cobalt chloride solution is 0.08-0.15 mol / L; the mass ratio of the material for completing the iron load, cobalt chloride and water is 10: 0.25-0.4: 80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h; in step (6), the concentration of the bismuth nitrate solution is 0.08-0.15 mol / L, the mass ratio of the material for completing the cobalt load, bismuth nitrate and water is 10 g: 0.08-0.15: 80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h.

[0044] In order to more specifically present the advantages and performance of the catalyst prepared by the present invention, the present invention provides the following examples for further description.

[0045] Example 1

[0046] A method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0047] (1) washing the rectorite with a 1 mol / L hydrochloric acid solution for 0.5 h at a dosage ratio of 1 g:10 mL, and then separating and washing to neutral treatment to obtain a pre-modified rectorite;

[0048] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide in a dosage ratio of 1:0.08 and treating the mixture at 800° C. for 2 h to obtain modified rectorite;

[0049] (3) mixing alumina and the modified rectorite obtained in step (2) in a mass ratio of 1:0.5, grinding and sieving through 200 mesh to obtain a composite carrier;

[0050] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0051] (5) adding the iron-loaded material in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0052] (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0053] Example 2

[0054] A method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0055] (1) washing the rectorite with a 1 mol / L hydrochloric acid solution for 0.5 h at a dosage ratio of 1 g:10 mL, and then separating and washing to neutral treatment to obtain a pre-modified rectorite;

[0056] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide in a dosage ratio of 1:0.08 and treating at 805° C. for 1.5 h to obtain modified rectorite;

[0057] (3) mixing alumina and the modified rectorite obtained in step (2) in a mass ratio of 1:0.55, grinding and sieving through 200 mesh to obtain a composite carrier;

[0058] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0059] (5) adding the iron-loaded material in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0060] (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0061] Example 3

[0062] A method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0063] (1) washing the rectorite with a 1 mol / L hydrochloric acid solution for 0.5 h at a dosage ratio of 1 g:10 mL, and then separating and washing to neutral treatment to obtain a pre-modified rectorite;

[0064] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide in a dosage ratio of 1:0.08 and treating the mixture at 800° C. for 2 h to obtain modified rectorite;

[0065] (3) mixing alumina and the modified rectorite obtained in step (2) in a mass ratio of 1:0.45, grinding and sieving through 200 mesh to obtain a composite carrier;

[0066] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0067] (5) adding the iron-loaded material in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0068] (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0069] Comparative Example 1

[0070] Compared with Example 1, Comparative Example 1 does not perform hydrochloric acid treatment on rectorite. Specifically, a method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0071] (1) Rectorite and sodium hydroxide are mixed in a dosage ratio of 1:0.08 and treated at 800°C for 2 hours. After the treatment, modified rectorite is obtained;

[0072] (2) mixing alumina and the modified rectorite obtained in step (1) in a mass ratio of 1:0.5, grinding and sieving through 200 mesh to obtain a composite carrier;

[0073] (3) adding the composite support obtained in step (2) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0074] (4) adding the iron-loaded material in step (3) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0075] (5) adding the cobalt-loaded material in step (4) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0076] Comparative Example 2

[0077] Compared with Example 1, the rectorite in Comparative Example 2 is not subjected to high-temperature treatment with sodium hydroxide. Specifically, a method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0078] (1) washing the rectorite with a 1 mol / L hydrochloric acid solution for 0.5 h at a dosage ratio of 1 g:10 mL, and then separating and washing to neutral treatment to obtain a pre-modified rectorite;

[0079] (2) mixing alumina and the pre-modified rectorite obtained in step (2) in a mass ratio of 1:0.5, grinding and sieving through 200 mesh to obtain a composite carrier;

[0080] (3) adding the composite support obtained in step (2) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0081] (4) adding the iron-loaded material in step (3) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0082] (5) adding the cobalt-loaded material in step (4) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0083] Comparative Example 3

[0084] Compared with Example 1, in Comparative Example 3, only alumina is used as a carrier, and the amount of alumina used is the same as the amount of alumina + rectorite used in Example 1. Specifically, a method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0085] (1) grinding and sieving alumina to 200 mesh to obtain a carrier;

[0086] (2) adding the carrier obtained in step (1) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the carrier, ferric chloride, and water is 10:0.6:120;

[0087] (3) adding the iron-loaded material in step (2) to a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to complete the cobalt loading; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100;

[0088] (4) adding the cobalt-loaded material in step (3) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining (545° C., 2 h) to obtain a catalyst product; wherein the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g:0.1:120.

[0089] Comparative Example 4

[0090] Compared with Example 1, in Comparative Example 4, bismuth is not loaded, that is, step (6) is omitted. Specifically, a method for preparing a catalyst for preparing carbon nanotubes comprises the following steps:

[0091] (1) washing the rectorite with a 1 mol / L hydrochloric acid solution for 0.5 h at a dosage ratio of 1 g:10 mL, and then separating and washing to neutral treatment to obtain a pre-modified rectorite;

[0092] (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide in a dosage ratio of 1:0.08 and treating the mixture at 800° C. for 2 h to obtain modified rectorite;

[0093] (3) mixing alumina and the modified rectorite obtained in step (2) in a mass ratio of 1:0.5, grinding and sieving through 200 mesh to obtain a composite carrier;

[0094] (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (540° C., 2.5 h) to complete the iron loading; wherein the mass ratio of the composite support, ferric chloride, and water is 10:0.6:120;

[0095] (5) adding the iron-loaded material in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining (535° C., 3 h) to obtain a catalyst product; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.35:100.

[0096] The catalysts prepared in Example 1 and Comparative Examples 1 to 4 were used to prepare carbon nanotubes in the following steps: the corresponding catalyst (10 g) was placed in a quartz glass tube reactor, and then nitrogen was introduced at a flow rate of 1.9 L / min for replacement;

[0097] Subsequently, the nitrogen was stopped and switched to a mixed gas (flow rate of 2.9 L / min) of ethylene, hydrogen and nitrogen (mixing ratio 2:0.3:1), and the quartz glass tube reactor was heated to 660°C. After 60 minutes of reaction, the heating and the methane gas were stopped. After cooling, carbon nanotubes were obtained. The amount of carbon nanotubes generated was counted, and the growth rate (carbon nanotubes generated / catalyst amount) was calculated; at the same time, a certain amount of carbon nanotubes was weighed and treated at a constant temperature of about 900°C in a muffle furnace for 3 hours, and then weighed again, and the mass loss was counted to obtain the ash content. The corresponding results are shown in Table 1.

[0098] Table 1

[0099] Growth rate Ash / % Example 1 19.24 2.56 Comparative Example 1 18.47 3.72 Comparative Example 2 17.85 3.98 Comparative Example 3 15.76 4.45 Comparative Example 4 13.54 5.73

[0100] It can be seen from Table 1 that the carbon nanotubes prepared in Example 1 of the present application have a high yield and a relatively high purity, indicating that the catalyst of the present application has a good catalytic effect.

[0101] The present invention illustrates the technical concept of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of individual raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a catalyst for preparing carbon nanotubes, It is characterized in that The steps include: (1) washing the rectorite with a hydrochloric acid solution, and then separating and washing it to a neutral state to obtain a pre-modified rectorite; (2) mixing the pre-modified rectorite obtained in step (1) with sodium hydroxide and subjecting the mixture to high temperature treatment, and obtaining modified rectorite after the treatment; (3) mixing the alumina and the modified rectorite obtained in step (2), grinding and sieving the mixture to obtain a composite carrier; (4) adding the composite support obtained in step (3) into a ferric chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the iron loading; (5) adding the material loaded with iron in step (4) into a cobalt chloride solution for impregnation, then adding water, stirring, drying, grinding, and calcining to complete the loading of cobalt; (6) adding the cobalt-loaded material in step (5) into a bismuth nitrate solution for impregnation, then adding water, stirring, drying, grinding, and calcining to obtain a catalyst product.

2. A method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (1), the concentration of the hydrochloric acid solution is 0.8-1.5 mol / L, and the dosage ratio of rectorite to the hydrochloric acid solution is 1 g: 5-15 mL.

3. The method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (2), the mass ratio of the pre-modified rectorite to sodium hydroxide is 1:0.01-0.1, the high temperature treatment temperature is 790-820°C, and the treatment time is 0.5-6h.

4. The method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (3), the mass ratio of alumina to modified rectorite is 1:0.3-0.6; and the sieve mesh number is 100-250 meshes.

5. The method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (4), the concentration of ferric chloride is 0.1-0.25 mol / L, the mass ratio of the composite carrier, ferric chloride and water is 10:0.4-0.8:80-150; the calcination temperature is 480-550°C, and the calcination time is 0.5-6h.

6. The method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (5), the concentration of the cobalt chloride solution is 0.08-0.15 mol / L; the mass ratio of the iron-loaded material, cobalt chloride, and water is 10:0.25-0.4:80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h.

7. The method for preparing a catalyst for preparing carbon nanotubes according to claim 1, It is characterized in that In step (6), the concentration of the bismuth nitrate solution is 0.08-0.15 mol / L, the mass ratio of the cobalt-loaded material, bismuth nitrate, and water is 10 g: 0.08-0.15: 80-150; the calcination temperature is 480-550° C., and the calcination time is 0.5-6 h.

8. A catalyst prepared by the method according to any one of claims 1 to 7.

9. Use of the catalyst according to claim 8 in preparing carbon nanotubes.

10. The use according to claim 9, It is characterized in that The preparation of carbon nanotubes comprises the following steps: placing the catalyst according to claim 8 in a quartz glass tube reactor, and then introducing nitrogen for replacement; Subsequently, the nitrogen gas is stopped and switched to a mixed gas of ethylene, hydrogen and nitrogen. The quartz glass tube reactor is heated to 620-800°C. After reacting for 0.5-6 hours, the heating and the methane gas are stopped. After cooling, carbon nanotubes are obtained.