Synthesis method of 2D / 2D ultrathin MoS2 / CdS nanosheet

2D/2D ultra-thin MoS2/CdS nanosheets were prepared through a one-step in-situ sulfurization + growth strategy, which solved the problems of poor stability and low photocatalytic activity of CdS materials, achieved efficient photocatalytic hydrogen production, and significantly improved the photocatalytic rate and Material stability.

CN118767948APending Publication Date: 2024-10-15CHINA THREE GORGES UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410839570.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

CdS photocatalytic materials have poor stability and low photocatalytic activity. It is difficult to prepare efficient and economical cocatalysts with existing technology, especially the preparation technology of hexagonal phase CdS nanosheets.

Method used

One-dimensional rod-shaped Mo3O10(C6H8N)2⋅2H2O is used as raw material and morphology inducer to prepare 2D/2D ultra-thin MoS2/CdS nanosheets through a one-step in-situ vulcanization + growth strategy. The two-dimensional nanosheet structure of MoS2 and CdS is used to increase the Large interface contact area promotes charge transfer.

Benefits of technology

Uniform dispersion and efficient photocatalysis of MoS2 and CdS nanosheets are achieved. The photocatalytic hydrogen production rate is significantly increased, surpassing the performance of pure CdS, and the material stability is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767948A_ABST
    Figure CN118767948A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method of a 2D / 2D ultrathin MoS2 / CdS nanosheet, and belongs to the field of nano material preparation. The 2D / 2D ultrathin MoS2 / CdS nanosheet is obtained by taking a one-dimensional organic-inorganic hybrid material Mo salt as a raw material and a morphology inducer and adopting a one-step in-situ vulcanization and growth strategy. And the thickness of the ultrathin nanosheet is 5 to 20 nm. The CdS prepared by the method is of a two-dimensional ultrathin nanosheet structure and is laminated and combined with the MoS2 nanosheets, and the CdS and the MoS2 nanosheets have a relatively large contact area, so that rapid transmission of charges is facilitated. Meanwhile, the method is simple, is mild in reaction condition, is economical and environment-friendly, is suitable for batch production, and has a good application prospect in the field of photocatalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for synthesizing a 2D / 2D ultra-thin MoS2 / CdS nanosheet, and belongs to the field of nano material preparation. Background Art

[0002] Traditional fossil energy reserves are limited, and the combustion products are not environmentally friendly and cannot meet the needs of sustainable development of human society. Therefore, the development and utilization of clean energy is urgent. Hydrogen energy is considered to be one of the most promising energy carriers in the future because of its clean and pollution-free characteristics. Photocatalytic decomposition of water to produce hydrogen can use solar energy and water to produce hydrogen, which is one of the most promising strategies to solve the energy crisis and environmental pollution. The preparation of efficient photocatalysts is a key way to promote the industrial application of photocatalytic decomposition of water to produce hydrogen.

[0003] Among the current photocatalytic materials, the most popular one in visible light responsive photocatalytic materials is CdS. CdS material has a suitable energy band structure and redox potential, which can absorb visible light and convert H + Reduction produces H2, making it the most promising semiconductor material. However, the recombination rate of photogenerated electrons and holes in CdS materials is relatively fast, and S 2- Under the action of photogenerated holes, it is easily oxidized into elemental S, thereby destroying the structure of the material and causing poor stability of the material. Therefore, the photocatalytic activity of CdS is low and it is easily corroded. Currently, loading the precious metal Pt on the surface of CdS is an effective way to improve the photocatalytic activity. However, the reserves of Pt on the earth are scarce and expensive, and there is an urgent need to prepare economical co-catalysts to improve the photocatalytic activity of CdS.

[0004] Most of the CdS that have been prepared so far are nanoparticles and nanorods, while two-dimensional nanosheet structure materials are widely used in energy storage and conversion due to their advantages such as fast electron transmission channels, more active sites and reduced agglomeration. At present, the preparation technology of hexagonal CdS nanosheets still faces great challenges. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing 2D / 2D ultrathin MoS2 / CdS nanosheets by using one-dimensional rod-shaped Mo3O 10 (C6H8N)2⋅2H2O is used as a raw material and a morphology inducing agent, and a simple in-situ sulfurization + growth strategy is used to achieve the preparation of 2D / 2D ultra-thin MoS2 / CdS nanosheets. In the 2D / 2D ultra-thin MoS2 / CdS nanosheets prepared by the present invention, both MoS2 and CdS are ultra-thin nanosheets, and the two are in contact through the sheet layer to form a larger interface contact, which is conducive to the rapid transmission of charges.

[0006] A method for preparing 2D / 2D ultrathin MoS2 / CdS nanosheets adopts a one-step in-situ sulfurization + growth strategy, comprising the following steps: 1) A certain amount of organic-inorganic hybrid molybdenum salt is ultrasonically dispersed in ethylenediamine solution.

[0007] 2) Add a sulfur source and a cadmium source to the above solution in proportion, stir and dissolve to obtain a mixed solution.

[0008] 3) The mixed solution is transferred to a hydrothermal reactor and reacted at a certain temperature for a period of time to obtain a precipitate.

[0009] 4) After the reaction is completed, the mixture is cooled to room temperature, washed with deionized water and anhydrous ethanol for three times respectively, and then dried in a vacuum drying oven to obtain 2D / 2D ultrathin MoS2 / CdS nanosheets.

[0010] Preferably, the organic-inorganic hybrid molybdenum salt is a one-dimensional rod-shaped Mo3O 10 (C6H8N)2⋅2H2O.

[0011] Preferably, the Mo3O 10 The concentration of (C6H8N)2⋅2H2O in ethylenediamine solution is 2-10 mmol / L.

[0012] Preferably, the sulfur source is thiourea or thioacetamide, and the cadmium source is cadmium nitrate or cadmium chloride.

[0013] Preferably, the molar ratio of thiourea to cadmium nitrate is 2:1-1:1, and the concentration of thiourea is 0.1-0.5 mol / L.

[0014] Preferably, the hydrothermal reaction temperature is 120-200° C., and the hydrothermal reaction time is 1-8 hours.

[0015] Compared with the prior art, the 2D / 2D ultrathin MoS2 / CdS nanosheets prepared by the present invention have the following beneficial effects: Both MoS2 and CdS are two-dimensional nanosheet structures, which are in contact with each other through stacking, forming a large contact area, providing a channel for rapid charge transfer. The nanosheets are evenly dispersed, which is conducive to exposing more active sites. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 : XRD spectrum of 2D / 2D ultrathin MoS2 / CdS nanosheets prepared in Example 1.

[0017] Figure 2 : This is a scanning electron microscope image of the 2D / 2D ultrathin MoS2 / CdS nanosheet prepared in Example 1.

[0018] Figure 3 : Photocatalytic hydrogen production effect of 2D / 2D ultrathin MoS2 / CdS nanosheets prepared in Example 1. DETAILED DESCRIPTION

[0019] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0020] Example 1 2 mmol (NH4)6Mo7O24‧4H2O was dissolved in 40 mL of deionized water and stirred to dissolve. 36 mmol C6H7N was added, followed by 1 M HCl dropwise. The pH value of the solution was adjusted to 4.0 and the reaction was carried out at 50 °C for 4 h to obtain one-dimensional rod-shaped Mo3O 10 (C6H8N)2⋅2H2O, washed with deionized water and anhydrous ethanol three times each, collected by centrifugation, and dried in a vacuum drying oven at 60°C overnight for later use.

[0021] Take 1.1 g and place it in Mo3O 10 (C6H8N)2⋅2H2O was ultrasonically dispersed in 32 mL of ethylenediamine solution, and then 1.7 g of thiourea was added and stirred evenly. Then 2 g of cadmium nitrate was added to dissolve to obtain a solution. The obtained mixed solution was placed in a hydrothermal reactor and reacted at 160°C for 2 h to obtain the product. The obtained product was washed with deionized water and dried to obtain 2D / 2D ultrathin MoS2 / CdS nanosheets. Figure 1 This is the XRD pattern of the 2D / 2D ultrathin MoS2 / CdS nanosheets obtained in this example. It can be seen from the figure that the product is mainly CdS, while the MoS2 content is low and the crystallinity is poor, so it cannot be observed in the XRD spectrum. Figure 2 This is a SEM image of the 2D / 2D ultrathin MoS2 / CdS nanosheet obtained in this example. It can be seen that the obtained product is a two-dimensional ultrathin nanosheet.

[0022] The 2D / 2D ultrathin MoS2 / CdS nanosheets of this example were used as photocatalysts for photocatalytic hydrogen production: 20 mg of 2D / 2D ultrathin MoS2 / CdS nanosheets were dispersed in 80 mL of a solution containing lactic acid (8 mL) and water (72 mL). A xenon lamp (MC-XF300) was used as a visible light source (λ ≥ 420 nm) to illuminate the reactor horizontally. Before illumination, the reactor was evacuated and a circulating cooling system was used to keep the temperature stable (7°C) during illumination. Using Ar as a carrier gas, the generated hydrogen was detected by gas chromatography every 1 h. Figure 3This is a diagram of the photocatalytic hydrogen production effect obtained in the experiment. From the figure, we can see that the photocatalytic hydrogen production rate of 2D / 2D ultrathin MoS2 / CdS nanosheets is 6.58 mmol / h / g, which is more than 10 times that of pure CdS (0.649 mmol / h / g). Example 2 Mo3O 10 The sample preparation of (C6H8N)2⋅2H2O was the same as in Example 1. 1.5 g was placed in Mo3O 10 (C6H8N)2⋅2H2O was ultrasonically dispersed in 40 mL of ethylenediamine solution, and then 1.5 g of thiourea was added and stirred evenly, and then 1.5 g of cadmium nitrate was added to dissolve to obtain a solution, and the obtained mixed solution was placed in a hydrothermal reactor, and reacted at 140°C for 2h to obtain a product, and the obtained product was washed with deionized water and dried to obtain 2D / 2D ultrathin MoS2 / CdS nanosheets. The 2D / 2D ultrathin MoS2 / CdS nanosheets of this embodiment were used as photocatalysts to carry out photocatalytic hydrogen production experiments, and the photocatalytic hydrogen production rate was 4.8 mmol / h / g, which is 7.4 times that of pure CdS.

[0023] Example 3 Mo3O 10 The sample preparation of (C6H8N)2⋅2H2O was the same as in Example 1. 1 g of the sample was placed in Mo3O 10 (C6H8N)2⋅2H2O was ultrasonically dispersed in 35 mL of ethylenediamine solution, and then 2 g of thiourea was added and stirred evenly, and then 2.5 g of cadmium nitrate was added to dissolve to obtain a solution, and the obtained mixed solution was placed in a hydrothermal reactor, and reacted at 140°C for 2h to obtain a product, and the obtained product was washed with deionized water and dried to obtain 2D / 2D ultrathin MoS2 / CdS nanosheets. The 2D / 2D ultrathin MoS2 / CdS nanosheets of this embodiment were used as photocatalysts to carry out photocatalytic hydrogen production experiments, and the photocatalytic hydrogen production rate was 7.56 mmol / h / g, which is 11.6 times that of pure CdS.

Claims

1. A 2D / 2D ultrathin MoS 2 / Synthesis method of CdS nanosheets, It is characterized in that The main steps include: (1) Ultrasonic dispersion of a certain amount of organic-inorganic hybrid molybdenum salt in ethylenediamine solution; (2) adding a sulfur source and a cadmium source to the above solution in order according to a certain ratio, stirring and dissolving them to obtain a mixed solution; (3) transferring the mixed solution to a hydrothermal reactor and reacting it at a certain temperature for a period of time to obtain a precipitate; (4) After the reaction, the mixture was cooled to room temperature, washed with water and anhydrous ethanol, and dried in a vacuum oven to obtain 2D / 2D ultrathin MoS 2 / CdS nanosheets.

2. The 2D / 2D ultrathin MoS according to claim 1 2 / Preparation method of CdS nanosheets, It is characterized in that The organic-inorganic hybrid molybdenum salt is a one-dimensional rod-shaped Mo 3 O 10 (C 6 H 8 N) 2 ⋅2H 2 O.

3. The 2D / 2D ultrathin MoS according to claim 1 2 / Preparation method of CdS nanosheets, It is characterized in that The Mo 3 O 10 (C 6 H 8 N) 2 ⋅2H 2 The concentration of O in EDTA solution is 2-10 mmol / L.

4. The 2D / 2D ultrathin MoS according to claim 1 2 / Preparation method of CdS nanosheets, It is characterized in that The sulfur source is thiourea or thioacetamide, and the cadmium source is cadmium nitrate or cadmium chloride.

5. The 2D / 2D ultrathin MoS according to claim 1 2 / Preparation method of CdS nanosheets, It is characterized in that The molar ratio of the thiourea to cadmium nitrate is 2:1-1:1, and the concentration of the thiourea is 0.1-0.5 mol / L.

6. The 2D / 2D ultrathin MoS according to claim 1 2 / Preparation method of CdS nanosheets, It is characterized in that The hydrothermal reaction temperature is 120-200° C., and the hydrothermal reaction time is 1-8 hours.

7. A 2D / 2D ultrathin MoS prepared by the preparation method of claims 1-6 2 / Application of CdS nanosheets in photocatalysis.

Citation Information

Patent Citations

  • One-dimensional nanometer photocatalyst as well as preparation method and application thereof

    CN103566953A

  • Composite photo-catalyst with molybdenum disulfide (MoS2) nanosheet / cadmium sulfide (CdS) nanowire core-shell structure

    CN105688945A

  • Preparation method and hydrogen production application of oxidation / reduction-double cocatalyst compounded CdS-based multi-element photocatalytic composite material

    CN111569909A

  • Three-dimensional composite material, preparation method thereof and application thereof in removal of water pollutants by visible light catalytic degrading

    US20190329233A1

  • Systems and methods for the production of tunable conductive molybdenum disulfide thin films

    US20220041463A1