Supported catalyst, preparation method thereof and propylene gas-phase epoxidation method

By loading a catalyst with a high content of zero-valent gold-tin alloy nanoparticles on a titanium-silicon molecular sieve, the problem of insufficient activity of the existing catalyst is solved, and the propylene conversion rate and propylene oxide selectivity of the propylene gas-phase epoxidation reaction are significantly improved, achieving Highly efficient catalytic performance.

CN118767985AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310373051.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

The existing Au/TS-1 catalyst has insufficient catalytic activity in the propylene gas-phase epoxidation reaction, resulting in a low propylene conversion rate. There is an urgent need to improve the catalytic performance of the catalyst.

Method used

Titanium-silicon molecular sieve is used as a carrier to load gold-tin alloy nanoparticles. The content of gold and tin elements is controlled to ensure that the proportion of zero-valent Au in the catalyst is higher than 90%. The particle size of the catalyst is optimized through specific preparation methods and conditions. and titanium to silicon molar ratio to improve catalytic activity.

Benefits of technology

The propylene conversion rate in the propylene gas-phase epoxidation reaction is significantly improved, and the propylene oxide selectivity reaches 85-95%, improving the overall performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767985A_ABST
    Figure CN118767985A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and discloses a supported catalyst, a preparation method and a propylene gas-phase epoxidation method. The catalyst comprises a titanium silicalite molecular sieve and gold-tin alloy nanoparticles loaded on the titanium silicalite molecular sieve, wherein on the basis of the total weight of the catalyst, the content of the gold element is 0.01-1 wt%, and the content of the tin element is 0.01-1 wt%; wherein the proportion of zero-valence Au in the gold element is greater than 95%. When the catalyst provided by the invention is used for catalyzing propylene gas-phase epoxidation reaction, the catalyst has relatively high catalytic activity, the propylene conversion rate is as high as 12-18%, and the epoxypropane selectivity can reach 85-95%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic chemistry and catalytic chemistry, and in particular to a supported catalyst and a preparation method thereof, and a method for gas-phase epoxidation of propylene. Background Art

[0002] Propylene oxide (PO) is one of the three major propylene derivatives, mainly used to produce organic chemical raw materials such as polyether polyols and propylene glycol. Polyurethane plastics produced from polyether polyols are essential materials for manufacturing daily necessities such as furniture, household appliances such as refrigerators, adhesives, sealants, etc. Propylene glycol can also be used in various fields related to people's lives, such as food, tobacco, cosmetics, and medicine. The chlorohydrin method for producing PO is the most mature process, with high product selectivity and low construction investment, but it has serious environmental pollution. The co-oxidation method for producing PO has a long process flow, high investment, and strict requirements on raw material quality, but its economic efficiency is restricted by the market supply and demand relationship of the co-product. The HPPO method uses TS-1 molecular sieve as a catalyst and H2O2 as an oxidant to prepare propylene oxide. The production process is green and efficient, but the supporting H2O2 production device will limit the process layout. For this reason, the propylene gas phase epoxidation route came into being. The gas phase epoxidation reaction is mild, highly selective, simple in process, green and environmentally friendly, clean and efficient.

[0003] Au / TS-1 catalyst has good catalytic activity for propylene gas phase epoxidation reaction. According to the mechanism of propylene gas phase epoxidation reaction, Au nanoparticles are the key active sites to promote the generation of H2O2. Studies have found that the Au nanoparticles deposited on the TS-1 carrier have various morphologies, and their catalytic activity is deeply affected by factors such as particle size, loading amount, loading position, and chemical state. The Au species deposited by DP method usually exist in ionic form on the TS-1 carrier (Au 1+ or Au 3+ Therefore, the Au / TS-1 catalyst must be activated to make the Au species present in the metallic state (Au 0 ) in order to play its catalytic role in the propylene gas phase epoxidation reaction. However, the catalytic activity of the Au / TS-1 catalyst in the prior art for the propylene gas phase epoxidation reaction cannot be further improved, especially the propylene conversion rate is low, so it is urgent to find a new catalyst to improve the catalytic activity of the propylene epoxidation catalyst. Summary of the invention

[0004] The purpose of the present invention is to overcome the problem that the catalytic performance of propylene epoxidation catalysts in the prior art for propylene gas phase epoxidation reaction is not high, and to provide a supported catalyst and a preparation method and a method for propylene gas phase epoxidation. When the supported catalyst provided by the present invention is used for propylene gas phase epoxidation reaction, the propylene conversion rate is significantly improved, and the supported catalyst has a high selectivity for propylene oxide.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a supported catalyst, which includes a titanium silicon molecular sieve and gold-tin alloy nanoparticles supported on the titanium silicon molecular sieve; wherein, based on the total weight of the catalyst, the content of gold element is 0.01-1% by weight, and the content of tin element is 0.01-1% by weight; wherein the proportion of zero-valent Au in the gold element is greater than 90%.

[0006] Preferably, based on the total weight of the catalyst, the content of gold is 0.04-0.8 wt %, and the content of tin is 0.04-0.8 wt %.

[0007] Preferably, in the catalyst, the particle size of the gold-tin alloy nanoparticles is less than 5 nm, preferably less than 3 nm.

[0008] Preferably, in the catalyst, the molar ratio of titanium to silicon is 0.005-0.04:1.

[0009] Preferably, the titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0010] The second aspect of the present invention provides a method for preparing the supported catalyst according to the first aspect, the method comprising the following steps:

[0011] S1, mixing an aqueous solution containing a gold compound and an aqueous solution containing a tin compound, and adjusting the pH value of the obtained mixed solution to alkaline to obtain an impregnation solution;

[0012] S2. Under stirring conditions, mixing the impregnation solution with the titanium silicon molecular sieve to react, then performing solid-liquid separation on the obtained reaction product, and activating the obtained solid product;

[0013] The amount of the gold-containing compound aqueous solution calculated as Au element is 0.05-5% by weight of the titanium silicon molecular sieve; the amount of the tin-containing compound aqueous solution calculated as Sn element is 0.05-5% by weight of the titanium silicon molecular sieve.

[0014] Preferably, in step S1, the gold compound aqueous solution is selected from one or more of an aqueous solution of chloroauric acid, an aqueous solution of cesium chloroaurate and an aqueous solution of potassium chloroaurate.

[0015] Preferably, in step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

[0016] Preferably, in step S1, the aqueous solution of the tin-containing compound is selected from one or more of an aqueous solution of tin tetrachloride, an aqueous solution of tin dichloride and an aqueous solution of dimethyltin.

[0017] Preferably, in step S1, the concentration of the aqueous solution of the tin-containing compound is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, more preferably 0.005-0.05 mol / L.

[0018] Preferably, in step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

[0019] Preferably, in step S1, the pH adjuster used to adjust the pH value of the mixture is an alkaline solution.

[0020] Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0021] Preferably, in step S2, the molar ratio of titanium to silicon in the titanium silicalite molecular sieve is 0.005-0.04:1.

[0022] Preferably, in step S2, the titanium silicon molecular sieve is selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0023] Preferably, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.1-5 weight % of the amount of the titanium silicon molecular sieve; the amount of the tin-containing compound aqueous solution calculated as Sn element is 0.1-5 weight % of the amount of the titanium silicon molecular sieve.

[0024] Preferably, in step S2, the reaction conditions include: temperature of 10-30° C., and time of 4-24 hours.

[0025] Preferably, in step S2, the activation conditions include: temperature of 150-300°C and time of 1-5 hours.

[0026] The third aspect of the present invention provides a supported catalyst prepared by the method described in the second aspect.

[0027] The fourth aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the supported catalyst described in the first aspect or the supported catalyst described in the third aspect.

[0028] Preferably, the reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1.

[0029] Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

[0030] Preferably, the reaction conditions include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa.

[0031] Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

[0032] The catalyst provided by the present invention adopts titanium silicon molecular sieve as a carrier, and gold-tin alloy nanoparticles are loaded on the carrier. The catalyst has a large amount of zero-valent gold, and the catalyst contains specific contents of gold and tin elements. The catalyst with these characteristics has high catalytic activity when catalyzing propylene gas phase epoxidation reaction, the propylene conversion rate is as high as 12-18%, and the propylene oxide selectivity can reach 85-95%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is the XPS spectra of the catalysts prepared in Example 1 and Comparative Example 1;

[0034] Figure 2 This is a HAADF-STEM image of the catalyst prepared in Example 1. DETAILED DESCRIPTION

[0035] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0036] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0037] The first aspect of the present invention provides a supported catalyst, which comprises a titanium silicon molecular sieve and gold-tin alloy nanoparticles supported on the titanium silicon molecular sieve.

[0038] In the present invention, the titanium in the titanium silicon molecular sieve and the tin in the gold-tin alloy nanoparticles can work together to improve the catalytic activity of the catalyst and significantly improve the propylene conversion rate. The inventors have found that Sn and Ti additives can jointly provide electrons to Au to obtain more electron-rich Au. 0 Active sites, thereby effectively promoting the rate-determining step of in-situ synthesis of H2O2 by hydrogen and oxygen, and having a high propylene conversion rate when applied to propylene gas-phase epoxidation reaction.

[0039] According to the present invention, the content of gold and tin in the catalyst has a great influence on improving the propylene conversion rate and propylene oxide selectivity when catalyzing the propylene gas phase epoxidation reaction. Wherein, based on the total weight of the catalyst, the content of gold can be 0.01-1% by weight, preferably 0.04-0.8% by weight; the content of tin can be 0.01-1% by weight, preferably 0.04-0.8% by weight.

[0040] In the present invention, the content of gold element and the content of tin element in the catalyst are measured by ICP.

[0041] According to the present invention, in order to improve the catalytic activity of the catalyst in the gas-phase epoxidation reaction of propylene, improve the propylene conversion rate and the selectivity of propylene oxide, the catalyst needs to have a higher proportion of zero-valent Au. Wherein, the proportion of zero-valent Au in the gold element is greater than 90%, which is detected and calculated by XPS.

[0042] In the present invention, XPS characterization obtains zero-valent Au (Au 0 ) The center position of the characteristic peak is located at 83-84eV; the peak area of ​​0-valent Au peak obtained by XPS peak software accounts for more than 90% of the total peak area. Among them, XPS measurement was carried out on the ESCALab250 X-ray photoelectron spectrometer of Thermo Fisher Scientific, with the excitation source being monochromatic Al Kα X-ray, energy of 1486.6eV, power of 150W; the penetration energy used for narrow scanning was 30eV; the basic vacuum during analysis was about 6.5×10 -8 Pa.

[0043] In the present invention, it is found that the particle size of the gold-tin alloy nanoparticles has a great influence on improving the catalytic effect of the catalyst. In order to improve the catalytic activity of the catalyst in the gas-phase epoxidation reaction of propylene, improve the propylene conversion rate and the selectivity of propylene oxide, preferably, in the catalyst, the particle size of the gold-tin alloy nanoparticles is less than 5nm, and more preferably less than 3nm. The particle size of the gold-tin alloy nanoparticles is obtained by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) observation.

[0044] In the present invention, in order to further improve the catalytic effect of the supported catalyst in the gas phase epoxidation reaction of propylene, preferably, in the catalyst, the titanium-silicon molar ratio is 0.005-0.04: 1. The titanium-silicon molar ratio is detected and calculated by an X-ray fluorescence spectrometer, wherein the instrument model is a ZSM Primus II X-ray fluorescence spectrometer of Rigaku Corporation, Japan, and the test conditions are a rhodium target, an excitation voltage of 40 kV, and an excitation current of 250 mA.

[0045] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0046] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0047] The second aspect of the present invention provides a method for preparing the supported catalyst according to the first aspect, the method comprising the following steps:

[0048] S1, mixing an aqueous solution containing a gold compound and an aqueous solution containing a tin compound, and adjusting the pH value of the obtained mixed solution to alkaline to obtain an impregnation solution;

[0049] S2. Under stirring conditions, the impregnation solution is mixed with the titanium silicon molecular sieve to react, and then the obtained reaction product is subjected to solid-liquid separation, and the obtained solid product is activated.

[0050] In the process of preparing the supported catalyst of the present invention, if the amount of the gold compound and the tin compound is too high, it will lead to the aggregation of metal nanoparticles, trigger side reactions during the propylene gas phase epoxidation reaction, and reduce the selectivity of propylene oxide; if the amount of the gold compound and the tin compound is too low, the catalytic activity of the prepared catalyst will be reduced. Therefore, it is necessary to control the amount of the gold compound and the tin compound so that an appropriate amount of gold-tin alloy nanoparticles can be loaded on the titanium silicon molecular sieve.

[0051] In the present invention, the amount of the gold-containing compound aqueous solution calculated as Au element is 0.05-5% by weight of the amount of the titanium silicon molecular sieve, preferably 0.1-5% by weight, for example, it can be 0.1% by weight, 0.5% by weight, 1% by weight, 1.5% by weight, 2% by weight, 2.5% by weight, 3% by weight, 3.5% by weight, 4% by weight, 4.5% by weight or 5% by weight.

[0052] In the present invention, the amount of the tin compound aqueous solution calculated as Sn element is 0.05-5% by weight of the amount of the titanium silicon molecular sieve, preferably 0.1-5% by weight, for example, it can be 0.1% by weight, 0.5% by weight, 1% by weight, 1.5% by weight, 2% by weight, 2.5% by weight, 3% by weight, 3.5% by weight, 4% by weight, 4.5% by weight or 5% by weight.

[0053] The present invention has no particular restrictions on the manner in which the gold-containing compound aqueous solution and the tin-containing compound aqueous solution are mixed. Preferably, the gold-containing compound aqueous solution and the tin-containing compound aqueous solution in the present invention can be mixed by stirring at room temperature. Similarly, adjusting the pH value of the obtained mixed solution to alkaline can also be achieved by stirring at room temperature.

[0054] In a preferred embodiment, the process of mixing the gold-containing compound aqueous solution and the tin-containing compound aqueous solution can be: firstly prepare the gold compound aqueous solution with water, prepare the tin compound aqueous solution with water, and then mix the gold compound aqueous solution and the tin compound aqueous solution to obtain a mixed solution. In this article, unless otherwise specified, room temperature refers to 20-30°C.

[0055] According to the present invention, the gold-containing compound aqueous solution can be a gold-containing compound aqueous solution well known to those skilled in the art. Preferably, in step S1, the gold-containing compound aqueous solution is selected from one or more of chloroauric acid aqueous solution, cesium chloroaurate aqueous solution and potassium chloroaurate aqueous solution.

[0056] In order to further improve the catalytic performance of the catalyst, improve the propylene conversion rate and propylene oxide selectivity, under preferred conditions, in step S1, the concentration of the gold compound aqueous solution can be 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

[0057] According to the present invention, the aqueous solution of the tin-containing compound can be an aqueous solution well known to those skilled in the art. Preferably, in step S1, the aqueous solution of the tin-containing compound is selected from one or more of an aqueous solution of tin tetrachloride, an aqueous solution of tin dichloride and an aqueous solution of dimethyltin.

[0058] In order to further improve the catalytic performance of the catalyst, improve the propylene conversion rate and propylene oxide selectivity, under preferred conditions, in step S1, the concentration of the tin compound aqueous solution can be 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, more preferably 0.005-0.05 mol / L.

[0059] In the present invention, in step S1, the pH value corresponding to the alkalinity may be 7-10, preferably 7-9, such as 7, 7.5, 8, 8.5 or 9.

[0060] In the present invention, specifically, the pH adjuster used to adjust the pH value of the mixture is an alkaline solution; the type and concentration of the alkaline solution are not specifically limited, as long as the pH value of the mixture can be adjusted to a specific alkalinity.

[0061] Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

[0062] According to the present invention, in order to further improve the catalytic activity and selectivity of the prepared catalyst, preferably, in step S1, the molar ratio of titanium to silicon in the titanium silicalite molecular sieve can be 0.005-0.04:1.

[0063] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0064] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0065] In the present invention, the titanium silicate molecular sieve can be purchased commercially, prepared according to the method in the prior art, or prepared by oneself.

[0066] In a specific embodiment of the present invention, in step (2), the entire process of mixing the impregnation solution with the titanium silicon molecular sieve for reaction is carried out under continuous stirring conditions, and the obtained reaction product is a suspension.

[0067] According to the present invention, specifically, the solid-liquid separation method of the reaction product obtained in step S2 can be various methods well known to those skilled in the art, as long as the solid product and the liquid can be separated. Preferably, the solid-liquid separation method is filtration or centrifugation.

[0068] According to the present invention, in order to further improve the propylene conversion rate and propylene oxide selectivity of the prepared supported catalyst in the propylene gas phase epoxidation reaction, preferably, in step S2, the reaction conditions include: the temperature is room temperature, specifically 10-30° C.; the time is 4-24 hours.

[0069] In some preferred embodiments of the present invention, in order to improve the catalytic performance of the catalyst in the propylene gas phase epoxidation reaction, and further improve the propylene conversion rate and propylene oxide selectivity, in step S2, the activation conditions include: a temperature of 150-300°C, for example, 150°C, 180°C, 200°C, 220°C, 250°C, 280°C or 300°C; a time of 1-5h, for example, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h. In a preferred embodiment, the activation process includes: calcination at 150-300°C in an air atmosphere for 1-5h.

[0070] The third aspect of the present invention provides a supported catalyst prepared by the method described in the second aspect.

[0071] In some preferred embodiments of the present invention, the catalyst comprises a titanium silicon molecular sieve and gold-tin alloy nanoparticles loaded on the titanium silicon molecular sieve; wherein, based on the total weight of the catalyst, the content of gold element is 0.01-1% by weight, and the content of tin element is 0.01-1% by weight; wherein the proportion of zero-valent Au in the gold element is greater than 90%.

[0072] In order to improve the catalytic performance of the catalyst, in the catalyst of the present invention, the particle size of the gold-tin alloy nanoparticles is less than 5 nm, and more preferably less than 3 nm. The particle size of the gold-tin alloy nanoparticles is obtained by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) observation.

[0073] Under preferred conditions, the molar ratio of titanium to silicon in the catalyst is 0.005-0.04:1.

[0074] According to the present invention, the type of the titanium silicon molecular sieve is not limited, as long as it is a molecular sieve containing silicon, titanium and oxygen.

[0075] In some preferred embodiments, the titanium silicalite molecular sieve may be selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

[0076] The catalyst prepared by the method of the present invention is used in catalyzing propylene gas phase epoxidation reaction, and the propylene conversion rate can reach 12-18%, and the propylene oxide selectivity can reach 85-95%.

[0077] The fourth aspect of the present invention provides a method for gas-phase epoxidation of propylene, the method comprising: in the presence of a protective gas and a catalyst, mixing hydrogen, oxygen and propylene for reaction to obtain propylene oxide; the catalyst is the supported catalyst described in the first aspect or the supported catalyst described in the third aspect.

[0078] According to the present invention, under preferred conditions, the reaction conditions include: the volume flow ratio of the hydrogen, oxygen and propylene is 0.5-2:0.5-2:1.

[0079] More preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10. In the present invention, the protective gas is nitrogen and / or an inert gas.

[0080] In some preferred embodiments of the present invention, the reaction conditions further include: temperature of 100-250° C. and pressure of 0.1-0.7 MPa; further preferably, temperature of 120-200° C. and pressure of 0.1-0.5 MPa.

[0081] In the present invention, the method for gas-phase epoxidation of propylene can be operated in a continuous manner. Specifically, after the catalyst is loaded into the reactor, a mixture of hydrogen, oxygen, propylene and protective gas is continuously added to carry out the reaction.

[0082] The present invention has no special requirements on the form of the catalyst. The catalyst may be in the form of powder or may be further loaded on a carrier for use. Those skilled in the art may select the catalyst according to the type of reactor.

[0083] In the present invention, the separation of the propylene gas-phase epoxidation product and the catalyst can be adjusted according to the form of the catalyst and actual needs. For example, when the catalyst is a powder, the product separation and the catalyst recovery and reuse can be achieved by sedimentation, filtration, centrifugation, evaporation, membrane separation, etc.; when the catalyst is a shaped catalyst supported on a carrier, the shaped catalyst can be loaded into a fixed bed reactor and the catalyst can be recovered after the reaction is completed.

[0084] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto. Unless otherwise specified, the raw materials used in the following examples are all chemically pure reagents.

[0085] In the present invention:

[0086] The contents of gold and tin in the catalyst were measured by inductively coupled plasma (ICP).

[0087] The particle size of Au-Sn alloy nanoparticles was observed by high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM).

[0088] The titanium-silicon molar ratio was analyzed by X-ray fluorescence spectrometry using a ZSM Primus II X-ray fluorescence spectrometer produced by Rigaku Corporation of Japan. The test conditions were a rhodium target, an excitation voltage of 40 kV, and an excitation current of 250 mA.

[0089] The proportion of zero-valent Au in the catalyst was detected and calculated by XPS. XPS determination was performed on an ESCALab250 X-ray photoelectron spectrometer from Thermo Fisher Scientific. The excitation source was monochromatic Al Kα X-rays with an energy of 1486.6 eV and a power of 150 W. The penetration energy used for narrow scanning was 30 eV. The basic vacuum during analysis was approximately 6.5×10 - 8 Pa.

[0090] Preparation Examples 1-3 are used to illustrate the preparation process of titanium silicalite molecular sieve.

[0091] Preparation Example 1 Preparation of TS-1 molecular sieve

[0092] About 3 / 4 of tetrapropylammonium hydroxide (TPAOH, 20%, purchased from Aldrich, USA) solution is added to tetraethyl orthosilicate (TEOS) solution to obtain a liquid mixture with a pH of about 13, and then the required amount of anhydrous isopropanol solution of n-butyl titanate [Ti(OBu)4] is added dropwise to the obtained liquid mixture under vigorous stirring. After stirring for 15 minutes, a clear liquid is obtained. Finally, the remaining TPAOH is slowly added to the clear liquid and stirred at 348-353K for about 3 hours to obtain a sol with a chemical composition of 0.03TiO2:SiO2:0.36TPA:35H2O. The sol is then crystallized at 443K for 3 days, and then the obtained solid is filtered, washed with distilled water, dried at 373K for 5 hours, and then calcined at 823K for 10 hours to obtain TS-1 molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TPAOH used is 73g, the amount of Ti(OBu)4 used is 2g, the amount of anhydrous isopropanol used is 10g, and the amount of water used is 68g.

[0093] Preparation Example 2 Preparation of TS-2 molecular sieve

[0094] A certain amount of tetrabutylammonium hydroxide solution (TBAOH, 20%) was mixed with tetraethyl orthosilicate (TEOS), and then the required amount of anhydrous isopropanol solution of n-butyl titanate [Ti(OBu)4] was added to the obtained transparent liquid mixture under vigorous stirring, and a clear liquid was obtained after stirring for 30 minutes for hydrolysis. Finally, 2 times the required amount of distilled water was added, and the obtained sol was stirred at 348-353K for 2h to remove alcohol. The chemical composition of the obtained sol is 0.03TiO2:SiO2:0.2TBA:20H2O. The sol was placed at 443K for crystallization for 3 days, and the obtained crystallized product was filtered, washed with water, and dried at 373K for 6h, and then calcined at 823K for 16h to obtain TS-2 molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TBAOH used is 52g, the amount of Ti(OBu)4 used is 2g, the amount of anhydrous isopropanol used is 10g, and the amount of water used is 30g.

[0095] Preparation Example 3 Preparation of Ti-Beta Molecular Sieve

[0096] A certain amount of tetraethyl orthosilicate (TEOS) is added to a solution of tetraethylammonium hydroxide solution (TEAOH, 20%) and hydrogen peroxide, and hydrolyzed for 2 hours under stirring. Then, a weighed anhydrous isopropanol solution of tetrabutyl titanate [Ti(OBu)4] is added to the hydrolyzed solution of tetrabutyl titanate, and stirring is continued for 3 hours to remove alcohol, and finally a sol with a chemical composition of TiO2: 60SiO2: 33TEA: 400H2O: 20H2O2 is obtained. Finally, the P-type molecular sieve seed after dealuminization is added and stirred vigorously (the amount of seed added is based on silica in the sol, and 4g seed is added to 100g silica). After the obtained mixture is crystallized at 413K for 14 days, the obtained slurry is filtered, washed with water, and dried at 373K for 6 hours, and then calcined at 823K for 12 hours to obtain Ti-Beta molecular sieve. Among them, the amount of TEOS used is 42g, the amount of TEAOH used is 81g, the amount of Ti(OBu)4 used is 1.16g, the amount of anhydrous isopropanol used is 10g, and the amount of hydrogen peroxide used is 7.5g.

[0097] Preparation Example 4

[0098] This preparation example is used to illustrate the preparation process of S-1 molecular sieve.

[0099] Tetrapropylammonium hydroxide (TPAOH, 20%, purchased from Aldrich, USA) solution was added to tetraethyl orthosilicate (TEOS) solution to obtain a liquid mixture with a pH of about 13, and stirred at 348-353K for about 3 hours to obtain a sol with a chemical composition of SiO2:0.36TPA:35H2O, and then crystallized at 443K for 3 days, after which the obtained solid was filtered, washed with distilled water, dried at 373K for 5 hours, and then calcined at 823K for 10 hours to obtain a molecular sieve sample. Among them, the amount of TEOS used was 42g, the amount of TPAOH used was 73g, and the amount of water used was 68g.

[0100] Test Example 1

[0101] The titanium-silicon molar ratio of the molecular sieves prepared in Preparation Examples 1-4 was detected and calculated, as shown in Table 1.

[0102] Table 1

[0103] serial number Molecular sieve number Mole ratio of titanium to silicon in molecular sieve Preparation Example 1 TS-1 0.025 Preparation Example 2 TS-2 0.027 Preparation Example 3 Ti-Beta 0.015 Preparation Example 4 S-1 /

[0104] Examples 1-10 and Comparative Examples 1-4 are used to illustrate the preparation process of the catalyst.

[0105] Example 1

[0106] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding sodium hydroxide solution to adjust the pH value of the obtained mixed solution to 7.7, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.03 mol / L;

[0107] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid to react at a reaction temperature of 20° C. for a reaction time of 6 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0108] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5% by weight of the amount of the TS-1 molecular sieve.

[0109] Example 2

[0110] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, and then adding potassium hydroxide solution to adjust the pH value of the obtained mixed solution to 8.1 to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.05 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.05 mol / L;

[0111] S2. Under continuous stirring conditions, TS-2 molecular sieves are added to the impregnation liquid for reaction at a reaction temperature of 22° C. for a reaction time of 8 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 180° C. for 2.5 h in an air atmosphere to obtain a catalyst;

[0112] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the amount of the TS-2 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5 weight % of the amount of the TS-2 molecular sieve.

[0113] Example 3

[0114] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, and then adding the cesium hydroxide solution to adjust the pH value of the obtained mixed solution to 8.2 to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.08 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.08 mol / L;

[0115] S2. Under continuous stirring conditions, adding Ti-Beta molecular sieve to the impregnation solution for reaction, the reaction temperature is 25° C., the reaction time is 10 h, and a suspension is obtained. The obtained suspension is then filtered, and the obtained filter residue is activated. The activation conditions include: calcining at 150° C. for 4 h in an air atmosphere to obtain a catalyst.

[0116] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5% by weight of the amount of the Ti-Beta molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5% by weight of the amount of the Ti-Beta molecular sieve.

[0117] Example 4

[0118] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding urea solution to adjust the pH value of the obtained mixed solution to 7.5, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.04 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.04 mol / L;

[0119] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid for reaction at a reaction temperature of 18° C. for a reaction time of 12 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 220° C. for 1.5 h in an air atmosphere to obtain a catalyst;

[0120] The amount of the chloroauric acid aqueous solution calculated as Au element is 3.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 3.5% by weight of the amount of the TS-1 molecular sieve.

[0121] Example 5

[0122] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, and then adding sodium carbonate solution to adjust the pH value of the obtained mixed solution to 8.3 to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.01 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.01 mol / L;

[0123] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid for reaction at a reaction temperature of 16° C. for a reaction time of 14 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 250° C. for 1 h in an air atmosphere to obtain a catalyst;

[0124] The amount of the chloroauric acid aqueous solution calculated as Au element is 1.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 1.5% by weight of the amount of the TS-1 molecular sieve.

[0125] Example 6

[0126] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding sodium bicarbonate solution to adjust the pH value of the obtained mixed solution to 7.1, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.01 mol / L;

[0127] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid to react at a reaction temperature of 14° C. for a reaction time of 16 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 250° C. for 3 h in an air atmosphere to obtain a catalyst;

[0128] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 0.1% by weight of the amount of the TS-1 molecular sieve.

[0129] Example 7

[0130] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding potassium bicarbonate solution to adjust the pH value of the obtained mixed solution to 8.8, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.04 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.09 mol / L;

[0131] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid for reaction at a reaction temperature of 12° C. for a reaction time of 18 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0132] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 4.5% by weight of the amount of the TS-1 molecular sieve.

[0133] Example 8

[0134] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding cesium carbonate solution to adjust the pH value of the obtained mixed solution to 7.2, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.008 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.05 mol / L;

[0135] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid for reaction at a reaction temperature of 10° C. for a reaction time of 20 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 180° C. for 3.5 h in an air atmosphere to obtain a catalyst;

[0136] The amount of the chloroauric acid aqueous solution calculated as Au element is 0.1% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5% by weight of the amount of the TS-1 molecular sieve.

[0137] Example 9

[0138] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding cesium bicarbonate solution to adjust the pH value of the obtained mixed solution to 8.9, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.05 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.002 mol / L;

[0139] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid for reaction at a reaction temperature of 25° C. for a reaction time of 4 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0140] The amount of the chloroauric acid aqueous solution calculated as Au element is 4.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5% by weight of the amount of the TS-1 molecular sieve.

[0141] Example 10

[0142] The method of Example 1 was followed, except that potassium carbonate solution was added to adjust the pH value of the resulting mixture.

[0143] Comparative Example 1

[0144] The method of Example 1 was followed, except that S-1 molecular sieve was used instead of TS-1 molecular sieve.

[0145] Comparative Example 2

[0146] The method of Example 1 is followed, except that no tin tetrachloride aqueous solution is added. The specific operation includes:

[0147] S1, adding sodium hydroxide solution to the chloroauric acid aqueous solution to adjust the pH value of the obtained mixed solution to 7.7 to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L;

[0148] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid to react at a reaction temperature of 25° C. for a reaction time of 6 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0149] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5 weight % of the amount of the TS-1 molecular sieve.

[0150] Comparative Example 3

[0151] The method of Example 1 is followed, except that the amount of the tin tetrachloride aqueous solution calculated as Sn element is 6% by weight of the amount of the TS-1 molecular sieve. The specific operations include:

[0152] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding sodium hydroxide solution to adjust the pH value of the obtained mixed solution to 7.7, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.03 mol / L;

[0153] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid to react at a reaction temperature of 25° C. for a reaction time of 6 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0154] The amount of the chloroauric acid aqueous solution calculated as Au element is 2.5% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 6% by weight of the amount of the TS-1 molecular sieve.

[0155] Comparative Example 4

[0156] The method of Example 1 is used, except that the amount of chloroauric acid aqueous solution calculated as Au element is 6% by weight of the amount of TS-1 molecular sieve. The specific operation includes:

[0157] S1, mixing the chloroauric acid aqueous solution and the tin tetrachloride aqueous solution uniformly, then adding sodium hydroxide solution to adjust the pH value of the obtained mixed solution to 7.7, to obtain an impregnation solution, wherein the concentration of the chloroauric acid aqueous solution is 0.03 mol / L, and the concentration of the tin tetrachloride aqueous solution is 0.03 mol / L;

[0158] S2. Under continuous stirring conditions, TS-1 molecular sieve is added to the impregnation liquid to react at a reaction temperature of 25° C. for a reaction time of 6 h to obtain a suspension, and then the obtained suspension is filtered and the obtained filter residue is activated. The activation conditions include: calcining at 200° C. for 2 h in an air atmosphere to obtain a catalyst;

[0159] The amount of the chloroauric acid aqueous solution calculated as Au element is 6% by weight of the amount of the TS-1 molecular sieve; the amount of the tin tetrachloride aqueous solution calculated as Sn element is 2.5% by weight of the amount of the TS-1 molecular sieve.

[0160] Test Example 2

[0161] The contents of Au and Sn in the catalysts prepared in Examples 1-10 and Comparative Examples 1-4 were tested, and the results are shown in Table 2. The test method is: according to the ASTM D5185 standard method, using SPECTRO ACROSS inductively coupled plasma (ICP) for determination.

[0162] XPS was used to detect the characteristic peak positions of Au elements in the catalysts prepared in Examples 1-10 and Comparative Examples 1-4, and the proportion of zero-valent Au was calculated. The results are shown in Table 2. The XPS spectra of the catalysts prepared in Example 1 and Comparative Example 1 are shown in Table 2. Figure 1 shown.

[0163] The molar ratio of titanium to silicon in the catalysts prepared in Examples 1-10 and Comparative Examples 1-4 was analyzed and calculated using X-ray fluorescence spectroscopy. The results are shown in Table 2.

[0164] The particle sizes of the gold-tin alloy nanoparticles in the catalysts prepared in Examples 1-10 and Comparative Examples 1-4 were observed by high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM), and the results are shown in Table 2. The high-angle annular dark field scanning transmission electron microscopy photo of the catalyst prepared in Example 1 is shown in Table 2. Figure 2 shown.

[0165] Table 2

[0166]

[0167]

[0168] Test Example 3

[0169] This test example is used to illustrate the reaction effect of the catalysts prepared in Examples 1-10 and Comparative Examples 1-4 of the present invention for the gas-phase epoxidation of propylene. The reagents used in this test example are all commercially available chemically pure reagents. The concentration of each substance after the reaction is quantitatively analyzed using gas chromatography. The instruments used are a 6890 gas chromatograph produced by Agilent, molecular sieve 5A and PoraBOND U chromatographic columns, and FID and TCD detectors.

[0170] In each embodiment and comparative example:

[0171] Propylene conversion % = (the number of moles of propylene in the feedstock - the number of moles of propylene in the product) / the number of moles of propylene in the feedstock × 100%;

[0172] Propylene oxide selectivity % = number of moles of propylene oxide in the product / total number of moles of the product × 100%.

[0173] The test process is as follows: the catalyst samples prepared in the above-mentioned embodiment and comparative example are taken respectively, loaded into a tubular reactor with an inner diameter of 8 mm, and then heated to 180°C in a N2 atmosphere, and hydrogen, oxygen, and propylene are introduced to start the reaction. After the reaction for 1 hour, the product is analyzed online; wherein, the amount of catalyst is 0.4 g, the flow rates of hydrogen, oxygen, propylene and nitrogen are 2 mL / min, 2 mL / min, 2 mL / min and 14 mL / min, respectively, the reaction pressure is 0.1 MPa, and the catalytic reaction results are shown in Table 3.

[0174] Table 3

[0175]

[0176]

[0177] As can be seen from Table 3, the propylene conversion rate of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is significantly higher than that of the comparative example, and the propylene oxide selectivity of the catalyst provided in the embodiment of the present invention for the propylene gas-phase epoxidation reaction is also maintained at a high level.

[0178] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A supported catalyst, characterized in that The catalyst comprises titanium silicon molecular sieve and gold-tin alloy nanoparticles loaded on the titanium silicon molecular sieve; Wherein, based on the total weight of the catalyst, the content of gold element is 0.01-1% by weight, and the content of tin element is 0.01-1% by weight; wherein the proportion of zero-valent Au in the gold element is greater than 90%.

2. The catalyst according to claim 1, characterized in that Based on the total weight of the catalyst, the content of gold element is 0.04-0.8 weight %, and the content of tin element is 0.04-0.8 weight %.

3. The catalyst according to claim 1 or 2, characterized in that In the catalyst, the particle size of the gold-tin alloy nanoparticles is less than 5 nm, preferably less than 3 nm.

4. The catalyst according to any one of claims 1 to 3, characterized in that In the catalyst, the molar ratio of titanium to silicon is 0.005-0.04:

1.

5. The catalyst according to claims 1-4, characterized in that The titanium silicon molecular sieve is one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

6. A method for preparing a supported catalyst, characterized in that: The method comprises the following steps: S1, mixing an aqueous solution containing a gold compound and an aqueous solution containing a tin compound, and adjusting the pH value of the obtained mixed solution to alkaline to obtain an impregnation solution; S2. Under stirring conditions, mixing the impregnation solution with the titanium silicon molecular sieve to react, then performing solid-liquid separation on the obtained reaction product, and activating the obtained solid product; The amount of the gold-containing compound aqueous solution calculated as Au element is 0.05-5% by weight of the titanium silicon molecular sieve; the amount of the tin-containing compound aqueous solution calculated as Sn element is 0.05-5% by weight of the titanium silicon molecular sieve.

7. The method according to claim 6, characterized in that In step S1, the gold compound aqueous solution is selected from one or more of an aqueous solution of chloroauric acid, an aqueous solution of cesium chloroaurate and an aqueous solution of potassium chloroaurate.

8. The method according to claim 6 or 7, characterized in that: In step S1, the concentration of the gold compound aqueous solution is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

9. The method according to any one of claims 6 to 8, characterized in that: In step S1, the tin compound aqueous solution is selected from one or more of a tin tetrachloride aqueous solution, a tin dichloride aqueous solution and a dimethyltin aqueous solution.

10. The method according to any one of claims 6 to 9, characterized in that: In step S1, the concentration of the aqueous solution of the tin compound is 0.0001-0.1 mol / L, preferably 0.0005-0.05 mol / L, and more preferably 0.005-0.05 mol / L.

11. The method according to any one of claims 6 to 10, characterized in that: In step S1, the pH value of the mixture is adjusted to 7-10, preferably 7-9.

12. The method according to any one of claims 6 to 11, characterized in that: In step S1, the pH adjusting agent used to adjust the pH value of the mixture is an alkaline solution; Preferably, the alkaline solution is selected from one or more of sodium hydroxide solution, potassium hydroxide solution, cesium hydroxide solution, urea solution, sodium carbonate solution, sodium bicarbonate solution, potassium carbonate solution, potassium bicarbonate solution, cesium carbonate solution and cesium bicarbonate solution.

13. The method according to any one of claims 6 to 12, characterized in that: In step S2, the molar ratio of titanium to silicon in the titanium silicate molecular sieve is 0.005-0.04:

1.

14. The method according to any one of claims 6 to 13, characterized in that: In step S2, the titanium silicon molecular sieve is selected from one or more of TS-1 molecular sieve, TS-2 molecular sieve, Ti-Beta molecular sieve and Ti-MWW molecular sieve.

15. The method according to any one of claims 6 to 14, characterized in that: The amount of the gold-containing compound aqueous solution calculated as Au element is 0.1-5 weight % of the amount of the titanium silicon molecular sieve; the amount of the tin-containing compound aqueous solution calculated as Sn element is 0.1-5 weight % of the amount of the titanium silicon molecular sieve.

16. The method according to any one of claims 6 to 15, characterized in that: In step S2, the reaction conditions include: temperature of 10-30°C and time of 4-24 hours.

17. The method according to any one of claims 6 to 16, characterized in that: In step S2, the activation conditions include: temperature of 150-300°C and time of 1-5h.

18. A supported catalyst prepared by the method of any one of claims 6 to 17.

19. A method for gas phase epoxidation of propylene, characterized in that: The method comprises: mixing hydrogen, oxygen and propylene for reaction in the presence of protective gas and catalyst to obtain propylene oxide; The catalyst is the supported catalyst according to any one of claims 1 to 5 or the supported catalyst according to claim 18.

20. The method according to claim 19, characterized in that The reaction conditions include: the volume flow ratio of hydrogen, oxygen and propylene is 0.5-2:0.5-2:1; Preferably, the volume flow rate ratio of propylene to protective gas is 1:1-10.

21. The method according to claim 19 or 20, characterized in that The reaction conditions include: temperature of 100-250°C and pressure of 0.1-0.7MPa; Preferably, the reaction conditions include: temperature of 120-220° C. and pressure of 0.1-0.5 MPa.

Citation Information

Patent Citations

  • Au / Ti-S catalyst as well as preparation method and application thereof

    CN111871447A

  • Preparation method of high-activity low-byproduct propylene gas-phase epoxidation catalyst

    CN112871205A

  • Hydrocarbon epoxidizing method

    CN1406909A