Leakage-proof phase-change energy storage wood with chitosan-based protective layer and preparation method of leakage-proof phase-change energy storage wood
By forming a chitosan-based protective layer on phase change energy storage wood, the problem of liquid leakage during the phase change process is solved, the anti-leakage properties are significantly improved, and the anti-leakage performance under high-temperature cycle conditions is ensured.
Patent Information
- Application Number
- CN202411084590.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Phase change energy storage wood has problems with liquid leakage during the phase change process, especially after multiple cycles of use, resulting in insufficient anti-leakage properties.
Using a chitosan-based protective layer, through delignification treatment, preparation of phase change energy storage liquid, sodium hydroxide treatment and electrostatic self-assembly technology, a multi-layer structure of leak-proof phase change energy storage wood is formed, which is fixed by the chitosan layer Phase change energy storage fluid enhances anti-leak properties.
After being placed on a 75°C hot stage for 10 hours and 200 heating and cooling cycles, the leakage-proof phase change energy storage wood did not leak phase change liquid, which significantly improved the leakage prevention performance of the phase change energy storage wood.
Smart Images

Figure CN118769337A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wood surface functional modification, and in particular relates to a leakage-proof phase-change energy storage wood with a chitosan-based protective layer and a preparation method thereof. Background Art
[0002] As energy crisis, environmental pollution and other problems become increasingly serious. Phase change energy storage materials are widely used in the field of thermal energy storage due to their characteristics of storing thermal energy through phase change, and play an important role in building temperature control, electronic component temperature control, textile temperature control and other fields. Phase change energy storage materials, especially organic solid-liquid phase change energy storage materials, are widely used due to their advantages of high phase change latent heat, good thermal reliability and thermal stability, no supercooling and no phase separation phenomenon, non-toxicity and non-corrosiveness. However, in practical applications, there is a major problem of liquid leakage during the phase change process. Wood has a unique anisotropic porous structure, with the advantages of excellent mechanical strength, degradability, low wood cost, wide sources and environmental friendliness. Combining wood with phase change energy storage materials, the capillary force of the hierarchical porous structure of wood can be used to solve the leakage problem of phase change energy storage materials during the phase change process. Unfortunately, after repeated cycles, phase change energy storage wood still leaks partially. Therefore, technological innovation is needed to further improve the anti-leakage characteristics of phase change energy storage wood. Summary of the invention
[0003] The problem to be solved by the present invention is to prepare leak-proof phase-change energy storage wood, and a leak-proof phase-change energy storage wood with a chitosan-based protective layer and a preparation method thereof are provided.
[0004] To achieve the above object, the present invention is implemented through the following technical solutions:
[0005] A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer comprises the following steps:
[0006] S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use;
[0007] S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use;
[0008] S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, repeating the above conditions 3-5 times, and then taking out and drying to obtain phase change energy storage wood for standby;
[0009] S4. Prepare a mixed solution of chitosan and acetic acid for standby use;
[0010] S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface;
[0011] Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
[0012] Furthermore, the method for delignification treatment in step S1 is to heat in a water bath at 75-80° C. according to the ratio of 2 g fast-growing wood pieces, 0.75-0.1 g NaClO2, 0.5-1 mL glacial acetic acid and 65-100 mL deionized water, and add 0.75 g NaClO2 and 0.5 mL glacial acetic acid every 1 hour for 3-5 times;
[0013] After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral;
[0014] The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
[0015] Furthermore, in step S2, the weight proportion of palmitic acid is 63-70 parts, the weight proportion of stearic acid is 37-45 parts, and the weight proportion of boron nitride is 1-1.5 parts. The palmitic acid and stearic acid are stirred at 80-85° C. for 0.5-1 h, and then boron nitride is added. The mixture is ultrasonically treated for 10-12 h in an ice-water bath, and the ultrasonic frequency is 75-100 Hz.
[0016] Furthermore, in step S3, the vacuum heating conditions are 60-65°C for 30 minutes under vacuum; the duration is 30 minutes under normal pressure; and the drying conditions are drying at room temperature for 5-10 minutes.
[0017] Furthermore, in step S4, the mixed solution of chitosan and acetic acid is prepared by adding 1-2 g of chitosan to 100 g of 1 wt % acetic acid aqueous solution, and stirring to obtain a mixed solution of chitosan and acetic acid.
[0018] Furthermore, the sodium hydroxide solution in step S5 is prepared by adding 5-10 mL of water to 2 g of NaOH and then adding 10-15 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 75-80° C. for 10-15 min.
[0019] Furthermore, in step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 20-30 minutes, the mixture is taken out and transferred to a 30-40° C. oven for drying for 20-30 minutes.
[0020] Furthermore, in step S5, the concentration of the hexagonal boron nitride nanosheet dispersion is 0.2-0.5wt%. After immersing in the hexagonal boron nitride nanosheet dispersion for 20-30 minutes, the mixture is transferred to a 30-40°C oven and dried for 5-10 minutes to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
[0021] A method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer. The leakage-proof phase-change energy storage wood with a chitosan-based protective layer is prepared. The leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multilayer structure.
[0022] Beneficial effects of the present invention:
[0023] The preparation method of a leakage-proof phase-change energy storage wood with a chitosan-based protective layer described in the present invention comprises the following steps: impregnating delignified wood with a phase-change solution composed of palmitic acid-stearic acid-boron nitride, then converting fatty acids into sodium fatty acids by sodium hydroxide treatment to obtain wood with a negatively charged surface, and finally coating the surface of the wood impregnated with the phase-change liquid with a positively charged chitosan layer by electrostatic self-assembly technology to obtain a leakage-proof phase-change energy storage wood. The introduction of the chitosan coating layer, as a supplement to the capillary force of the hierarchical porous structure of the wood, fixes the phase-change energy storage liquid in the wood frame, further enhancing the leakage-proof properties of the phase-change energy storage wood. The leakage-proof phase-change energy storage wood obtained by the present invention is placed on a 75°C hot stage for 10 hours without leakage of the phase-change liquid. In addition, the leakage-proof phase-change energy storage wood obtained did not leak after 200 heating and cooling cycles at 75°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a flow chart of a method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer according to the present invention;
[0025] Figure 2 The SEM photo of the leakage-proof phase-change energy storage wood with a chitosan-based protective layer prepared by the present invention and the element content distribution diagram corresponding to each layer, wherein a is the SEM photo of the leakage-proof phase-change energy storage wood with a chitosan-based protective layer, and b is the element content distribution diagram corresponding to each layer;
[0026] Figure 3 Comparative photos of leakage experiments conducted under different temperature conditions on the phase change energy storage wood prepared by the present invention and the leakage-proof phase change energy storage wood with a chitosan-based protective layer, wherein a is the phase change energy storage wood, and b is the leakage-proof phase change energy storage wood with a chitosan-based protective layer. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the specific embodiments described are only part of the embodiments of the present invention, rather than all of the specific embodiments. The components of the specific embodiments of the present invention described and shown in the drawings herein can be arranged and designed in various different configurations, and the present invention can also have other embodiments.
[0028] Therefore, the following detailed description of the specific embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected specific embodiments of the present invention. Based on the specific embodiments of the present invention, all other specific embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.
[0029] In order to further understand the content, features and effects of the present invention, the following specific implementation methods are given as examples, and the attached Figure 1 -Attached Figure 3 The detailed instructions are as follows:
[0030] Embodiment 1:
[0031] A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer comprises the following steps:
[0032] S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use;
[0033] Furthermore, the method for delignification treatment in step S1 is to heat the mixture in a water bath at 75° C. according to the ratio of 2 g of fast-growing wood sheet, 0.75 g of NaClO2, 0.5 mL of glacial acetic acid and 65 mL of deionized water, and add 0.75 g of NaClO2 and 0.5 mL of glacial acetic acid every 1 h for 3 times;
[0034] After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral;
[0035] The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
[0036] S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use;
[0037] Furthermore, in step S2, the weight proportion of palmitic acid is 63 parts, the weight proportion of stearic acid is 37 parts, and the weight proportion of boron nitride is 1 part. The palmitic acid and stearic acid are stirred at 80° C. for 0.5 h, and then boron nitride is added. The mixture is ultrasonicated in an ice-water bath for 12 h, and the ultrasonic frequency is 75 Hz.
[0038] S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, after repeating the above conditions 3 times, take out and dry to obtain phase change energy storage wood, set aside;
[0039] Furthermore, in step S3, the vacuum heating condition is 60°C for 30 minutes under vacuum; the duration is 30 minutes under normal pressure; the drying condition is drying at room temperature for 5 minutes;
[0040] S4. Prepare a mixed solution of chitosan and acetic acid for standby use;
[0041] Furthermore, in step S4, the mixed solution of chitosan and acetic acid is prepared by adding 1 g of chitosan to 100 g of 1 wt% acetic acid aqueous solution, and stirring to obtain a mixed solution of chitosan and acetic acid;
[0042] S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface;
[0043] Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
[0044] Furthermore, the sodium hydroxide solution in step S5 is prepared by adding 2 g of NaOH to 5 mL of water and then to 10 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 75° C. for 10 min.
[0045] Furthermore, in step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 20 minutes, the mixture is taken out and transferred to a 30° C. oven for drying for 20 minutes.
[0046] Furthermore, in step S5, the concentration of the hexagonal boron nitride nanosheet dispersion is 0.2 wt %. After immersing in the hexagonal boron nitride nanosheet dispersion for 20 min, the mixture is transferred to a 30° C. oven and dried for 5 min to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
[0047] Furthermore, the fast-growing wood used in step S1 is balsa wood chips, and the thickness of the wood chips is 1-4 mm.
[0048] The method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer described in this embodiment is a method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer. The leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multilayer structure, such as Figure 2 As shown, from Figure 2 It can be seen that a phase change energy storage wood with a negatively charged surface (9μm thick) can be obtained by NaOH treatment, which provides conditions for the subsequent introduction of a chitosan layer by layer electrostatic self-assembly technology. On this basis, a chitosan layer (16μm thick) was successfully coated on the surface of the phase change energy storage wood. At the same time, in order not to affect the phase change characteristics of the phase change energy storage wood, a boron nitride layer with a thickness of about 0.2μm was also coated on the outside of the chitosan layer. Combining Figures a and b, it can be seen that a phase change energy storage wood with a negatively charged surface can be obtained by NaOH treatment, which provides conditions for the subsequent introduction of a chitosan layer by layer electrostatic self-assembly technology. On this basis, a chitosan layer (16μm thick) was successfully coated on the surface of the phase change energy storage wood. At the same time, in order not to affect the phase change characteristics of the phase change energy storage wood, a boron nitride layer with a thickness of about 0.2μm was also coated on the outside of the chitosan layer.
[0049] The method for preparing a leak-proof phase-change energy storage wood with a chitosan-based protective layer described in this embodiment prepares a leak-proof phase-change energy storage wood with a chitosan-based protective layer. The introduction of the chitosan coating layer, as a supplement to the capillary force of the hierarchical porous structure of the wood, fixes the phase-change energy storage liquid in the wood frame, further enhancing the leak-proof properties of the phase-change energy storage wood. Figure 3As shown, by comparing Figure a and Figure b, it can be seen that at 25°C, both phase change energy storage woods will not leak the phase change liquid. However, after the phase change energy storage wood was placed on a 75°C hot stage for 10 hours, obvious phase change liquid leakage was observed, while the anti-leakage phase change energy storage wood with a chitosan-based protective layer did not leak the phase change liquid. Therefore, this embodiment is effective in improving the anti-leakage properties of the phase change energy storage wood by constructing a chitosan-based protective layer. In addition, the obtained anti-leakage phase change energy storage wood did not leak after 200 heating and cooling cycles at 75°C.
[0050] The method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer described in this embodiment is a leakage-proof phase-change energy storage wood having a chitosan-based protective layer. The performance comparison is shown in Table 1:
[0051] Table 1:
[0052]
[0053]
[0054] It can be seen from Table 1 that the introduction of the chitosan protective layer does not have a significant effect on the melting temperature, melting phase change enthalpy, solidification temperature, and solidification phase change enthalpy of the phase change energy storage wood. Therefore, the introduction of the chitosan protective layer can enhance the anti-leakage properties of the sample without weakening the energy storage properties of the phase change energy storage wood.
[0055] Embodiment 2:
[0056] A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer comprises the following steps:
[0057] S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use;
[0058] Furthermore, the method for delignification treatment in step S1 is to heat 2 g of fast-growing wood pieces, 0.1 g of NaClO2, 1 mL of glacial acetic acid and 100 mL of deionized water in a water bath at 80° C., and add 0.75 g of NaClO2 and 0.5 mL of glacial acetic acid every 1 hour for 5 times;
[0059] After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral;
[0060] The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
[0061] S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use;
[0062] Furthermore, in step S2, the weight proportion of palmitic acid is 70 parts, the weight proportion of stearic acid is 45 parts, and the weight proportion of boron nitride is 1.5 parts. The palmitic acid and stearic acid are stirred at 85° C. for 0.5 h, and then boron nitride is added. The mixture is ultrasonicated in an ice-water bath for 12 h, and the ultrasonic frequency is 100 Hz.
[0063] S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, after repeating the above conditions 5 times, take out and dry to obtain phase change energy storage wood, set aside;
[0064] Furthermore, in step S3, the vacuum heating condition is 65°C for 30 minutes under vacuum; the duration is 30 minutes under normal pressure; the drying condition is drying at room temperature for 10 minutes;
[0065] S4. Prepare a mixed solution of chitosan and acetic acid for standby use;
[0066] Furthermore, in step S4, the mixed solution of chitosan and acetic acid is prepared by adding 2 g of chitosan to 100 g of 1 wt% acetic acid aqueous solution, and stirring to obtain a mixed solution of chitosan and acetic acid;
[0067] S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface;
[0068] Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
[0069] Furthermore, the sodium hydroxide solution in step S5 is prepared by adding 2 g of NaOH to 10 mL of water and then to 15 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 80° C. for 15 minutes.
[0070] Furthermore, in step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 30 minutes, the mixture is taken out and transferred to a 40° C. oven for drying for 30 minutes.
[0071] Furthermore, in step S5, the concentration of the hexagonal boron nitride nanosheet dispersion is 0.5wt%. After immersing in the hexagonal boron nitride nanosheet dispersion for 30 minutes, the mixture is transferred to a 30-40°C oven and dried for 10 minutes to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
[0072] The method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer described in this embodiment prepares a leakage-proof phase-change energy storage wood with a chitosan-based protective layer, and the leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multi-layer structure.
[0073] Embodiment 3:
[0074] A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer comprises the following steps:
[0075] S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use;
[0076] Furthermore, the method for delignification treatment in step S1 is to heat the mixture in a water bath at 75° C. according to the ratio of 2 g of fast-growing wood pieces, 0.8 g of NaClO2, 0.6 mL of glacial acetic acid and 70 mL of deionized water, and add 0.75 g of NaClO2 and 0.5 mL of glacial acetic acid every 1 h for 4 times;
[0077] After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral;
[0078] The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
[0079] S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use;
[0080] Furthermore, in step S2, the weight proportion of palmitic acid is 65 parts, the weight proportion of stearic acid is 40 parts, and the weight proportion of boron nitride is 1 part. The palmitic acid and stearic acid are stirred at 80° C. for 0.5 h, and then boron nitride is added. The mixture is ultrasonicated in an ice-water bath for 12 h, and the ultrasonic frequency is 80 Hz.
[0081] S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, after repeating the above conditions 4 times, take out and dry to obtain phase change energy storage wood, set aside;
[0082] Furthermore, in step S3, the vacuum heating condition is 60°C for 30 minutes under vacuum; the duration is 30 minutes under normal pressure; the drying condition is drying at room temperature for 10 minutes;
[0083] S4. Prepare a mixed solution of chitosan and acetic acid for standby use;
[0084] Furthermore, the mixed solution of chitosan and acetic acid in step S4 is prepared by adding 1.5 g of chitosan to 100 g of 1 wt% acetic acid aqueous solution, and stirring to obtain a mixed solution of chitosan and acetic acid;
[0085] S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface;
[0086] Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
[0087] Furthermore, the sodium hydroxide solution in step S5 is prepared by adding 2 g of NaOH to 5 mL of water and then to 12 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 75° C. for 10 min.
[0088] Furthermore, in step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 20 minutes, the mixture is taken out and transferred to a 35° C. oven for drying for 25 minutes.
[0089] Furthermore, in step S5, the concentration of the hexagonal boron nitride nanosheet dispersion is 0.3 wt %. After immersing in the hexagonal boron nitride nanosheet dispersion for 20 min, the mixture is transferred to a 35° C. oven and dried for 5 min to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
[0090] The method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer described in this embodiment prepares a leakage-proof phase-change energy storage wood with a chitosan-based protective layer, and the leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multi-layer structure.
[0091] Embodiment 4:
[0092] A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer comprises the following steps:
[0093] S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use;
[0094] Furthermore, the method for delignification treatment in step S1 is to heat the mixture in a water bath at 75° C. according to the ratio of 2 g of fast-growing wood sheet, 0.9 g of NaClO2, 0.9 mL of glacial acetic acid and 80 mL of deionized water, and add 0.75 g of NaClO2 and 0.5 mL of glacial acetic acid every 1 h for 5 times;
[0095] After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral;
[0096] The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
[0097] S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use;
[0098] Furthermore, in step S2, the weight proportion of palmitic acid is 63 parts, the weight proportion of stearic acid is 37 parts, and the weight proportion of boron nitride is 1 part. The palmitic acid and stearic acid are stirred at 80° C. for 0.5 h, and then boron nitride is added. The mixture is ultrasonicated in an ice-water bath for 10 h, and the ultrasonic frequency is 75 Hz.
[0099] S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, after repeating the above conditions 3 times, take out and dry to obtain phase change energy storage wood, set aside;
[0100] Furthermore, in step S3, the vacuum heating condition is 60°C for 30 minutes under vacuum; the duration is 30 minutes under normal pressure; the drying condition is drying at room temperature for 10 minutes;
[0101] S4. Prepare a mixed solution of chitosan and acetic acid for standby use;
[0102] Furthermore, in step S4, the mixed solution of chitosan and acetic acid is prepared by adding 1 g of chitosan to 100 g of 1 wt% acetic acid aqueous solution, and stirring to obtain a mixed solution of chitosan and acetic acid;
[0103] S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface;
[0104] Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
[0105] Furthermore, the sodium hydroxide solution in step S5 is prepared by adding 2 g of NaOH to 5 mL of water and then to 10 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 75° C. for 10 min.
[0106] Furthermore, in step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 20-30 minutes, the mixture is taken out and transferred to a 30° C. oven for drying for 20 minutes.
[0107] Furthermore, in step S5, the concentration of the hexagonal boron nitride nanosheet dispersion is 0.4 wt %. After immersing in the hexagonal boron nitride nanosheet dispersion for 20 min, the mixture is transferred to a 30° C. oven and dried for 5 min to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
[0108] The method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer described in this embodiment prepares a leakage-proof phase-change energy storage wood with a chitosan-based protective layer, and the leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multi-layer structure.
[0109] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0110] Although the present application has been described above with reference to specific embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, as long as there is no structural conflict, the various features in the specific embodiments disclosed in the present application may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer, characterized in that: The steps include: S1. Preparation and modification of delignified wood: a mixed solution of NaClO2 and glacial acetic acid was used to delignify the fast-growing wood, the treated fast-growing wood was immersed and washed in distilled water until the pH value of the distilled water was neutral, and then taken out and freeze-dried to obtain delignified wood for standby use; S2. Preparation of phase change energy storage liquid: Weigh a certain weight of palmitic acid, stearic acid and boron nitride in parts by weight, dissolve palmitic acid and stearic acid at a certain temperature, then add boron nitride, and ultrasonicate for a certain time in an ice water bath to obtain a phase change energy storage liquid for standby use; S3. Phase change energy storage wood preparation, the delignified wood obtained in step S1 is immersed in the phase change energy storage liquid prepared in step S2, and then heated under vacuum conditions for a certain period of time and then under normal pressure conditions for a certain period of time, repeating the above conditions 3-5 times, and then taking out and drying to obtain phase change energy storage wood for standby; S4. Prepare a mixed solution of chitosan and acetic acid for standby use; S5. Preparation of a leak-proof phase change energy storage wood having a chitosan-based protective layer, wherein the phase change energy storage wood obtained in step S3 is placed in a sodium hydroxide solution for a certain period of time to obtain a phase change energy storage wood having a negative charge on the surface; Then, the mixture is placed in the mixed solution of chitosan and acetic acid obtained in step S4 and vacuum immersed for a certain period of time. After being taken out and dried, the mixture is placed in a dispersion of hexagonal boron nitride nanosheets and immersed for a certain period of time. After being taken out and dried, a leakage-proof phase change energy storage wood with a chitosan-based protective layer is obtained.
2. The method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer according to claim 1, characterized in that: The method for delignification treatment in step S1 is to heat 2 g of fast-growing wood pieces, 0.75-0.1 g of NaClO2, 0.5-1 mL of glacial acetic acid and 65-100 mL of deionized water in a water bath at 75-80° C., and add 0.75 g of NaClO2 and 0.5 mL of glacial acetic acid every 1 hour for 3-5 times; After the reaction is completed, soak and wash in distilled water, and change the distilled water every half an hour until the pH value of the distilled water is neutral; The conditions for freeze drying are vacuum degree less than 10Pa and temperature below -50°.
3. The method for preparing a leakage-proof phase-change energy storage wood with a chitosan-based protective layer according to claim 1 or 2, characterized in that: In step S2, the weight proportion of palmitic acid is 63-70 parts, the weight proportion of stearic acid is 37-45 parts, and the weight proportion of boron nitride is 1-1.5 parts. The palmitic acid and stearic acid are stirred at 80-85° C. for 0.5-1 h, and then boron nitride is added. The mixture is ultrasonically treated for 10-12 h in an ice-water bath, and the ultrasonic frequency is 75-100 Hz.
4. The method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer according to claim 3, characterized in that: In step S3, the vacuum heating conditions are 60-65° C. for 30 min under vacuum and 30 min under normal pressure; and the drying conditions are drying at room temperature for 5-10 min.
5. The method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer according to claim 4, characterized in that: The method for preparing the mixed solution of chitosan and acetic acid in step S4 is to add 1-2 g of chitosan to 100 g of 1 wt % acetic acid aqueous solution, and stir evenly to obtain the mixed solution of chitosan and acetic acid.
6. The method for preparing a leakage-proof phase-change energy storage wood having a chitosan-based protective layer according to claim 5, characterized in that: The sodium hydroxide solution in step S5 is prepared by adding 5-10 mL of water to 2 g of NaOH and then adding 10-15 mL of ethanol; the phase change energy storage wood obtained in step S3 is placed in the sodium hydroxide solution and treated at 75-80° C. for 10-15 minutes.
7. The method for preparing the leak-proof phase-change energy storage wood with a chitosan-based protective layer according to claim 6, characterized in that: In step S5, after vacuum impregnation in the mixed solution of chitosan and acetic acid for 20-30 minutes, the mixture is taken out and transferred to a 30-40° C. oven for drying for 20-30 minutes.
8. The method for preparing the leakage-proof phase-change energy storage wood with a chitosan-based protective layer according to claim 7, characterized in that: The concentration of the hexagonal boron nitride nanosheet dispersion in step S5 is 0.2-0.5wt%. After immersing in the hexagonal boron nitride nanosheet dispersion for 20-30 minutes, the mixture is transferred to a 30-40°C oven and dried for 5-10 minutes to obtain a leakage-proof phase change energy storage wood with a chitosan-based protective layer.
9. A method for preparing a leak-proof phase-change energy storage wood having a chitosan-based protective layer. A leak-proof phase-change energy storage wood having a chitosan-based protective layer is prepared, characterized in that: The leakage-proof phase-change energy storage wood with a chitosan-based protective layer has a multi-layer structure.
Citation Information
Patent Citations
Leak-proof gel low-temperature phase change material and preparation method thereof
CN106433568A
Preparation method and application of charcoal-based shaped composite phase change energy storage material
CN118185574A
Manufacturing device / method of surface layer-modified wood material
JP2008307798A