Modified spinel type metal oxide as well as preparation method and application thereof
By plasma etching spinel-type metal oxides, a modified catalyst is formed, which solves the problem of slow reaction in the OER process of electrolyzing water to produce hydrogen, and achieves efficient and low-cost hydrogen production by electrolyzing water.
Patent Information
- Application Number
- CN202410810265.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-15
AI Technical Summary
In the process of electrolyzing water to produce hydrogen, the oxygen evolution reaction (OER) process of the anode requires a high overpotential and the reaction is slow, which limits the hydrogen production efficiency. Commonly used precious metal catalysts are expensive and difficult to apply on a large scale.
By plasma etching spinel-type metal oxides, a modified catalyst is formed, which increases the oxygen vacancies in the catalyst, optimizes the interaction between the catalyst and reactants, and improves OER activity and conductivity.
It achieves excellent oxygen evolution catalytic reaction activity at a lower overpotential, improves the efficiency of the water electrolysis hydrogen production process, reduces costs, and is easy to produce on a large scale.
Smart Images

Figure CN118771464A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of green hydrogen production by electrolysis of water, and specifically relates to a modified spinel metal oxide and a preparation method and application thereof. Background Art
[0002] With the development of social economy, energy and environmental issues have received increasing attention. Hydrogen energy is considered to be one of the ideal clean energy sources in the 21st century due to its high energy density, green and pollution-free, abundant reserves, wide application, and the ability to be effectively coupled with clean energy such as wind energy, electricity, and solar energy.
[0003] Among many hydrogen production technologies, water electrolysis is regarded as a highly promising renewable energy hydrogen production technology because of its advantages of high hydrogen purity and green and pollution-free process. Generally, the process of water electrolysis involves two half-reaction processes, namely the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Both half-reaction processes involve electron transfer. However, the OER process is a multi-step electron transfer process compared to the HER process, which requires a higher overpotential, and the reaction is slower and more difficult, limiting the hydrogen production efficiency of the entire water electrolysis process. Currently, most commonly used oxygen evolution catalysts are precious metals or precious metal oxides. Although these catalysts can exhibit good OER characteristics, precious metal elements such as Ir, Pt, and Ru are the main factors limiting the large-scale development and application of such catalysts in OER reactions. Therefore, it is urgent to develop efficient, stable, and low-cost catalysts to replace such precious metal catalysts, reduce the reaction energy barrier of the OER process, and accelerate the OER reaction rate to achieve the improvement of the efficiency of the entire water electrolysis hydrogen production process.
[0004] Metal oxides containing transition metal elements, especially transition metal oxides with spinel structure, have gradually shown great application prospects and value in the field of electrocatalysis. Among them, spinel metal oxides containing Fe, Co, Ni, Mn and Cu have a huge structural modification space and performance controllability due to their unique AB2O4 structure, but they still have the disadvantage of poor catalytic performance when applied to OER reactions. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a modified spinel metal oxide and a preparation method and application thereof. The modified spinel metal oxide provided by the present invention can exhibit excellent oxygen evolution catalytic reaction activity in a water electrolysis hydrogen production reaction system as an oxygen evolution catalyst.
[0006] In order to achieve the above object, the present invention provides the following scheme:
[0007] The present invention provides a method for preparing a modified spinel metal oxide, comprising the following steps:
[0008] Plasma etching the spinel metal oxide to obtain a modified spinel metal oxide;
[0009] The plasma etching time is 10 to 40 minutes.
[0010] Preferably, the atmosphere of the plasma etching includes an argon-oxygen mixed atmosphere or a nitrogen-oxygen mixed atmosphere.
[0011] Preferably, the volume ratio of argon to oxygen in the argon-oxygen mixed atmosphere is (1-2):(1-3); and the volume ratio of nitrogen to oxygen in the nitrogen-oxygen mixed atmosphere is (1-2):(1-3).
[0012] Preferably, the spinel metal oxide is composed of AB2O4, wherein the metal element A is Cu, Co or Ni; and the metal element B is Mn, Co, Cr, Al or Fe.
[0013] Preferably, the method for preparing the spinel metal oxide comprises the following steps:
[0014] Mixing a salt of metal element A and a salt of metal element B, a chelating agent, a dispersant and a solvent to obtain a sol solution;
[0015] Subjecting the sol solution to self-propagating combustion to obtain a metal oxide precursor;
[0016] calcining the metal oxide precursor to obtain a spinel metal oxide;
[0017] The molar ratio of the metal element A to the metal element B is 1:2.
[0018] Preferably, the salt of metal element A and the salt of metal element B are independently one or more of nitrate, sulfate, chloride and acetate.
[0019] Preferably, the mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the chelating agent is (1-6):(2-4); the mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the dispersant is (1-6):(1-3); the volume ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the solvent is (1-6) g:(20-30) mL.
[0020] Preferably, the calcination temperature is 500-900° C. and the calcination time is 2-3 hours.
[0021] The present invention provides a modified spinel-type metal oxide prepared by the preparation method described in the above scheme.
[0022] The present invention provides the use of the modified spinel metal oxide described in the above scheme as an oxygen evolution catalyst in hydrogen production by electrolysis of water.
[0023] The invention provides a method for preparing a modified spinel metal oxide, comprising the following steps: plasma etching the spinel metal oxide to obtain the modified spinel metal oxide; the plasma etching time is 10 to 40 minutes.
[0024] In the OER catalytic material system, the method of regulating the oxygen-rich vacancies of the material through defect engineering (i.e., plasma etching in the present invention) can make the catalyst (i.e., spinel metal oxide) exhibit better OER performance. Specifically, plasma etching constructs oxygen vacancies in the catalyst, that is, using high-energy plasma to bombard the metal oxide catalyst, which can effectively eliminate oxygen atoms in the metal oxide catalyst, so that the metal oxide catalyst produces more oxygen vacancies. Oxygen vacancies in the catalyst can greatly change the interaction process between the catalyst and the reactants. On the one hand, the formation of oxygen vacancies in the catalyst can induce coordination unsaturated metal sites, reduce the adsorption energy of intermediates, thereby optimizing the adsorption process of oxygen intermediates, and may simplify the adsorption mechanism, so that the OER activity of the catalyst is enhanced; on the other hand, oxygen vacancies can expose more metal active sites in the catalyst, resulting in an increase in the catalyst reaction active area. In addition, oxygen vacancies in the catalyst can act as electron donors, driving delocalized electrons to excite to the conduction band to increase the charge carrier density, thereby improving the conductivity of the catalyst material.
[0025] The method provided by the present invention can realize the plasma etching modification of the spinel oxygen evolution catalyst (spinel metal oxide), and the modified spinel oxygen evolution catalyst can show excellent oxygen evolution catalytic reaction activity in the water electrolysis hydrogen production reaction system, and has strong practicality and application value.
[0026] In addition, the preparation and modification method of the high-performance spinel oxygen evolution catalyst provided by the present invention has a simple process, low equipment requirements, cheap and readily available raw materials, and is easy to achieve large-scale production. It can be used as an oxygen evolution catalyst in an electrolyzer for electrolyzing water to produce green hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0028] Figure 1 A flow chart of the preparation, plasma modification and realization of high-efficiency electrocatalytic oxygen evolution reaction of the spinel-type high-performance oxygen evolution catalyst provided by the present invention;
[0029] Figure 2 This is a physical picture of the metal oxide precursor powder formed by the dry gel in Example 1 by self-propagating combustion;
[0030] Figure 3 XRD spectra of spinel metal oxide CoMn2O4 powders prepared at different calcination temperatures in Examples 1 to 5;
[0031] Figure 4 This is a physical picture of the catalyst-containing ink dispersion prepared by 600-CMO@20min obtained in Example 1;
[0032] Figure 5 This is a physical picture of the catalytic electrode prepared by 600-CMO@20min obtained in Example 1;
[0033] Figure 6 XRD spectra of bare nickel foam (NF), nickel foam loaded 600-CMO catalyst sample (600-CMO / NF), and nickel foam loaded 600-CMO@20min catalyst sample (600-CMO@20min / NF) in Example 1;
[0034] Figure 7 SEM morphology images of NF (a), 600-CMO / NF (b) and 600-CMO@20min / NF (c) in Example 1;
[0035] Figure 8 The distribution diagram of Ni, Co, Mn and O elements in the 600-CMO@20min / NF sample in Example 1;
[0036] Fig. 9 LSV curves of NF, 600-CMO / NF and 600-CMO@20min / NF in Example 1;
[0037] Fig.10 The Tafel curves of NF, 600-CMO / NF and 600-CMO@20min / NF in Example 1;
[0038] Fig.11 is the C of NF, 600-CMO / NF and 600-CMO@20min / NF in Example 1 dl curve;
[0039] Fig.12These are the EIS curves of NF, 600-CMO / NF and 600-CMO@20min / NF in Example 1. DETAILED DESCRIPTION
[0040] The present invention provides a method for preparing a modified spinel metal oxide, comprising the following steps:
[0041] The spinel metal oxide is plasma etched to obtain a modified spinel metal oxide.
[0042] Unless otherwise specified, the materials and equipment used in the present invention are commercially available.
[0043] In the present invention, the composition of the spinel metal oxide is preferably AB2O4, wherein the metal element A is Cu, Co or Ni; and the metal element B is Mn, Co, Cr, Al or Fe.
[0044] In the present invention, the method for preparing the spinel metal oxide preferably comprises the following steps:
[0045] Mixing a salt of metal element A and a salt of metal element B, a chelating agent, a dispersant and a solvent to obtain a sol solution;
[0046] Subjecting the sol solution to self-propagating combustion to obtain a metal oxide precursor;
[0047] The metal oxide precursor is calcined to obtain a spinel metal oxide.
[0048] The present invention mixes a metal salt, a chelating agent, a dispersant and a solvent to obtain a sol solution;
[0049] The molar ratio of the metal element A to the metal element B is 1:2.
[0050] In the present invention, the salt of the metal element A and the salt of the metal element B are independently preferably one or more of nitrate, sulfate, chloride and acetate. Specifically, when the metal element is Cu, the corresponding salt is copper nitrate, copper sulfate, copper chloride or copper acetate; when the metal element is Co, the corresponding salt is cobalt nitrate, cobalt sulfate, cobalt chloride or cobalt acetate; when the metal element is Ni, the corresponding salt is nickel nitrate, nickel sulfate, nickel chloride or nickel acetate; when the metal element is Mn, the corresponding salt is manganese nitrate, manganese sulfate, manganese chloride or manganese acetate; when the metal element is Cr, the corresponding salt is chromium nitrate, chromium sulfate, chromium chloride or chromium acetate; when the metal element is Al, the corresponding salt is aluminum nitrate, aluminum sulfate, aluminum chloride or aluminum acetate; when the metal element is Fe, the corresponding salt is iron nitrate, iron sulfate, iron chloride or iron acetate.
[0051] In the present invention, the chelating agent is preferably one of ethylenediamine, monoethanolamine, diethanolamine, triethanolamine, ethylenediaminetetraacetic acid, aminotriacetic acid, tartaric acid, citric acid, oxalic acid and sulfosalicylic acid.
[0052] In the present invention, the dispersant is preferably one of polyethylene glycol 200, polyethylene glycol 300, polyethylene glycol 400, polyethylene glycol 600, polyethylene glycol methyl ether, polymethyl acrylate, polyvinyl pyrrolidone, maleic anhydride, methyl cellulose and carboxymethyl cellulose.
[0053] In the present invention, the solvent is preferably a mixed solvent of ethanol and water or ethanol. In the present invention, when the solvent is a mixed solvent of ethanol and water, the volume ratio of ethanol to water is preferably (5-9):1, more preferably (6-8):1.
[0054] In the present invention, the mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the chelating agent is preferably (1-6): (2-4), and more preferably (2-4): (2.5-3.5); the mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the dispersant is preferably (1-6): (1-3), and more preferably (2-4): (1.5-2.5); the volume ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the solvent is preferably (1-6) g: (20-30) mL, and more preferably (2-3) g: (22-25) mL.
[0055] In the present invention, the mixing temperature is preferably 25 to 30° C., more preferably 25° C.; the mixing time is preferably 2 to 3 hours, more preferably 2 hours; and the mixing is preferably performed under stirring.
[0056] After the mixing is completed, the present invention preferably adjusts the pH value of the obtained mixed solution to neutral to prevent metal ion precipitation. If the solution is alkaline or acidic, it will cause metal ion precipitation (different metal ion precipitation values are different), ultimately resulting in an impure spinel metal oxide phase.
[0057] After obtaining the sol solution, the present invention performs self-propagating combustion on the sol solution to obtain a metal oxide precursor.
[0058] When the solvent is a mixed solvent of ethanol and water, the present invention preferably dries the sol solution before the self-propagating combustion.
[0059] In the present invention, the drying temperature is preferably 50 to 60° C., more preferably 52 to 58° C.; the drying time is preferably 1 to 2 hours, more preferably 1.5 to 2 hours.
[0060] The present invention has no special requirements for the self-propagating combustion method, and any method known in the art may be used.
[0061] Self-propagating combustion uses the heat released by the combustion reaction of the original chemical reaction raw materials to make the chemical reaction process continue spontaneously. In the self-propagating combustion process, metal salts containing transition metal elements (such as cobalt nitrate and manganese nitrate) and chelating agents (such as citric acid) undergo combustion reactions in the form of oxidants and reductants respectively, while chelating agents and dispersants (such as polyethylene glycol 200) act as combustion aids to provide energy support for the combustion reaction. The heat released by the combustion reaction causes the redox reaction of the metal salt and the chelating agent to continue, and finally the organic compounds in the reaction system are burned out to obtain a metal oxide precursor.
[0062] After obtaining the metal oxide precursor, the present invention calcines the metal oxide precursor to obtain a spinel metal oxide.
[0063] In the present invention, the calcination temperature is preferably 500-900°C, more preferably 550-800°C, and more preferably 600-750°C; the calcination time is preferably 2-3h, more preferably 2.5-2.8h; the calcination atmosphere is preferably an air atmosphere; the calcination is preferably heated from room temperature to the calcination temperature, and the heating rate is preferably 5°C / min.
[0064] In the calcination process of the present invention, the metal oxide precursor is melted under high temperature conditions to form daughter crystals, which continuously receive the metal oxide melt under high temperature conditions and finally develop and grow into spinel oxygen evolution catalysts (spinel metal oxides).
[0065] After obtaining the spinel metal oxide, the present invention performs plasma etching on the spinel metal oxide to obtain a modified spinel metal oxide.
[0066] In the present invention, the atmosphere of the plasma etching preferably includes an argon-oxygen mixed atmosphere or a nitrogen-oxygen mixed atmosphere; the volume ratio of argon and oxygen in the argon-oxygen mixed atmosphere is preferably (1-2):(1-3), and more preferably (1.5-1.8):(1.5-2.5); in the nitrogen-oxygen mixed atmosphere, the volume ratio of nitrogen and oxygen is preferably (1-2):(1-3), and more preferably (1.5-1.8):(1.5-2.5).
[0067] In the present invention, the plasma etching time is 10 to 40 minutes, preferably 15 to 35 minutes, and more preferably 20 to 30 minutes.
[0068] The present invention modifies spinel metal oxides by plasma etching, and bombards metal oxide catalysts with high-energy plasma, which can effectively eliminate oxygen atoms in metal oxide catalysts, so that the metal oxide catalysts produce more oxygen vacancies. The oxygen vacancies in the catalyst (i.e., spinel metal oxide) can greatly change the interaction process between the catalyst and the reactants. On the one hand, the formation of oxygen vacancies in the catalyst can induce coordination unsaturated metal sites, reduce the adsorption energy of intermediates, thereby optimizing the adsorption process of oxygen intermediates, and may simplify the adsorption mechanism, so that the OER activity of the catalyst is enhanced; on the other hand, oxygen vacancies can expose more metal active sites in the catalyst, resulting in an increase in the catalyst reaction active area. In addition, the oxygen vacancies in the catalyst can act as electron donors, driving delocalized electrons to excite to the conduction band to increase the charge carrier density, thereby improving the conductivity of the catalyst material.
[0069] The preparation method provided by the present invention is easy to operate, has high feasibility, strong practicality, and the raw materials are easily available, easy to mass produce, and low in cost, and can bring considerable economic benefits to the development and utilization of the green hydrogen production technology industry by electrolysis of water.
[0070] The present invention provides a modified spinel-type metal oxide prepared by the preparation method described in the above scheme.
[0071] The present invention provides the use of the modified spinel metal oxide described in the above scheme as an oxygen evolution catalyst in hydrogen production by electrolysis of water.
[0072] The present invention has no special requirements for the application method, and a method well known in the art can be used. In the present invention, specifically, a modified spinel metal oxide is used as an oxygen evolution catalyst to prepare a catalyst-containing ink, and then the ink is ultrasonically dispersed and drop-coated on a nickel foam, and after drying, an oxygen evolution electrode loaded with a modified spinel catalyst is obtained.
[0073] In the present invention, the ultrasonic dispersion time is preferably 1 to 3 hours; the drying temperature is preferably 60 to 70° C., and the drying time is preferably 2 to 3 hours.
[0074] The oxygen evolution electrode loaded with a modified spinel catalyst provided by the present invention can exhibit excellent electrocatalytic oxygen evolution characteristics at a relatively low overpotential.
[0075] Figure 1 The present invention provides a flow chart for the preparation of a spinel-type high-performance oxygen evolution catalyst, plasma modification, and realization of a highly efficient electrocatalytic oxygen evolution reaction. Figure 1As shown, the present invention utilizes a self-propagating combustion method to obtain a metal oxide precursor, which is then calcined to obtain a spinel-type oxygen evolution catalyst CoMn2O4, and the synthesized spinel-type oxygen evolution catalyst is further etched by plasma to obtain a modified spinel-type oxygen evolution catalyst. Finally, the modified spinel-type oxygen evolution catalyst is formulated into a catalyst-containing ink, and the catalyst-containing ink is ultrasonically dispersed and then drop-coated on nickel foam, and after drying, an oxygen evolution electrode loaded with a modified spinel catalyst is obtained, which can exhibit excellent electrocatalytic oxygen evolution reaction at a relatively low overpotential.
[0076] In order to further illustrate the present invention, a modified spinel metal oxide provided by the present invention and its preparation method and application are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0077] Example 1
[0078] 15.76 g of citric acid monohydrate and 14 g of polyethylene glycol 200 were added to a mixed solution of 200 mL of ethanol and water (the volume ratio of ethanol to water was 9:1), and magnetic stirring was performed at 25° C. After the citric acid monohydrate in the mixed solution was completely dissolved, 13.32 g of cobalt nitrate hexahydrate and 29.88 g of manganese nitrate aqueous solution (the mass of manganese nitrate accounted for 50% of the mass of the manganese nitrate aqueous solution) were added to the mixed solution, and the molar ratio of metal cobalt ions to metal manganese ions in the solution was maintained at 1:2. The mixed solution was then stirred for 2 h at 25° C. After the metal salt was completely dissolved, the pH value of the mixed solution was adjusted to neutral with ammonia water to form a dark green sol solution;
[0079] Drying the sol solution at 60° C. for 2 h to obtain a dry gel;
[0080] The dry gel was ignited in the air using a few drops of anhydrous ethanol, and the dry gel burned rapidly in a self-propagating manner to form a gray metal oxide precursor powder (see the actual picture). Figure 2 shown);
[0081] The metal oxide precursor powder is ground and placed in a programmed temperature furnace, heated from room temperature to 600° C., and calcined for 2 hours at a heating rate of 5° C. / min to obtain a powder, namely CoMn2O4 spinel metal oxide, recorded as 600-CMO.
[0082] The XRD diffraction peaks of CoMn2O4 spinel metal oxide powder are completely consistent with the diffraction peaks of spinel CoMn2O4 ( Figure 3 ), which indicates that CoMn2O4 spinel metal oxide was successfully prepared by the self-propagating combustion method combined with the calcination method under low temperature conditions (low temperature calcination compared to the traditional calcination temperature).
[0083] The CoMn2O4 spinel metal oxide (600-CMO) was placed in a plasma etcher and etched for 20 minutes in a mixed atmosphere of Ar and O2 with a volume ratio of 1:1 to obtain a modified spinel metal oxide, which was recorded as 600-CMO@20min.
[0084] Embodiments 2 to 5
[0085] The preparation steps are the same as those in Example 1, except that the calcination temperatures are 500°C, 700°C, 800°C, and 900°C, respectively.
[0086] The XRD diffraction peaks of the CoMn2O4 spinel metal oxide powders prepared by different calcination temperatures in Examples 2 to 5 are completely consistent with the diffraction peaks of the spinel CoMn2O4 ( Figure 3 As shown), this indicates that CoMn2O4 spinel metal oxide was successfully prepared under low temperature conditions by self-propagating combustion method combined with calcination method.
[0087] Performance Testing
[0088] The 600-CMO and 600-CMO@20min etching samples prepared in Example 1 were respectively used as catalysts to prepare inks and then drop-coated on nickel foam for performance testing. The specific steps are as follows:
[0089] Nickel foam loaded 600-CMO@20min catalyst sample (600-CMO@20min / NF): 10 mg of 600-CMO@20min etched sample, 100 μL of deionized water, 100 μL of ethanol, and 5 μL of Nafion solution were prepared into ink containing catalyst. The prepared ink was ultrasonicated at room temperature for 2 h to obtain ink dispersion (see the actual picture). Figure 4 Then, the ink dispersion was coated on the nickel foam sheet (the size of the rectangular nickel foam was 1×2 cm) by the method of drip coating and drying, and the coating area was 1×1 cm. Then, the oxygen evolution electrode was prepared by drying at 70°C for 2 h (as shown in the actual picture). Figure 5 (shown in the middle right figure).
[0090] Nickel foam loaded 600-CMO catalyst sample (600-CMO / NF): The preparation steps are the same as those of nickel foam loaded 600-CMO@20min catalyst sample, the only difference is that the catalyst sample is 600-CMO.
[0091] Comparison of XRD spectra of bare nickel foam (NF), nickel foam loaded 600-CMO catalyst sample (600-CMO / NF), and nickel foam loaded 600-CMO@20min catalyst sample (600-CMO@20min / NF) Figure 6 As shown in Figure 3, it can be found that the diffraction peaks of the 600-CMO / NF sample and the 600-CMO / NF@20min sample are consistent with the characteristic diffraction peaks of spinel CoMn2O4 (PDF#00-055-0685), which indicates that plasma etching does not change the crystal phase structure of spinel CoMn2O4.
[0092] Compared with NF( Figure 7 a), 600-CMO / NF( Figure 7 b) and 600-CMO@20min / NF( Figure 7 SEM morphology of (c) Figure 7 As shown in Figure 2, it can be found that the pores of NF can be fully filled by 600-CMO sample and 600-CMO@20min, and the 600-CMO@20min / NF sample prepared by plasma etching 600-CMO catalyst shows a rougher surface ( Figure 7 c), which further demonstrates that plasma can etch the CMO catalyst, and the rough surface of the 600-CMO@20min / NF sample helps improve the oxygen evolution reaction characteristics of the catalyst. In addition, the element distribution diagram of the 600-CMO@20min / NF sample shows that Ni, Co, Mn, and O are evenly distributed ( Figure 8 shown).
[0093] Oxygen evolution reaction is a key step in the production of hydrogen by water electrolysis. Therefore, oxygen evolution catalysts have a crucial impact on the efficiency of hydrogen production by water electrolysis. The oxygen evolution catalytic performance of the prepared catalysts was evaluated and tested under a three-electrode system. Linear sweep voltammetry ( Fig. 9 The test results show that at 10mA / cm -2 At a current density of 100 mA / cm, the overpotential of 600-CMO@20min / NF is 367 mV, which is significantly lower than that of NF (overpotential of 554 mV) and 600-CMO / NF (overpotential of 383 mV). 2 Under the condition of , the overpotential of 600-CMO / NF@20min is only 479mV, which is significantly lower than that of NF (overpotential is 759mV) and 600-CMO / NF (overpotential is 522mV). It can be seen that the 600-CMO / NF@20min sample has better oxygen evolution reaction characteristics.
[0094] The Tafel slope can reflect the change in the electrocatalytic reaction rate on the electrode. The smaller the Tafel slope, the better the oxygen evolution reaction kinetics of the electrode. The Tafel curve test results of NF, 600-CMO / NF and 600-CMO@20min / NF show that the Tafel slope of the 600-CMO / NF@20min sample is 105.88mV / dec, which is significantly lower than the Tafel slope of 179.41mV / dec of the NF sample and the Tafel slope of 128.35mV / dec of the 600-CMO / NF sample ( Fig.10 Therefore, the 600-CMO / NF@20min sample exhibits more excellent kinetic properties.
[0095] The ECSA can usually be calculated by using the electrical double layer capacitance (C dl ) for comparison, C dl The larger the value, the larger the ECSA, the higher the electrocatalytic activity of the catalytic electrode, and the better the electrochemical performance. dl The C value of 600-CMO@20min / NF can be found dl Value (0.968mF / cm 2 ) is higher than NF's C dl Value (0.332mF / cm 2 ) and 600-CMO / NF C dl Value (0.935mF / cm 2 ). Therefore, the 600-CMO@20min / NF sample exhibits better electrocatalytic activity ( Fig.11 shown).
[0096] In electrochemical impedance spectroscopy (EIS), R ct Represents the charge transfer of electrochemical reactions, R ct The smaller the value, the faster the charge transfer rate during the electrochemical reaction and the better the electrochemical performance of the catalyst. ct R of 44.25Ω, 600-CMO / NF ct is 30.53Ω, while the R ct Only 24.81Ω( Fig.12 Therefore, the 600-CMO / NF@20min sample has a more excellent conductivity.
[0097] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a modified spinel metal oxide, characterized in that: The following steps are involved: Plasma etching the spinel metal oxide to obtain a modified spinel metal oxide; The plasma etching time is 10 to 40 minutes.
2. The preparation method according to claim 1, characterized in that: The plasma etching atmosphere includes an argon-oxygen mixed atmosphere or a nitrogen-oxygen mixed atmosphere.
3. The preparation method according to claim 2, characterized in that: The volume ratio of argon to oxygen in the argon-oxygen mixed atmosphere is (1-2):(1-3); the volume ratio of nitrogen to oxygen in the nitrogen-oxygen mixed atmosphere is (1-2):(1-3).
4. The preparation method according to claim 1, characterized in that: The spinel metal oxide is composed of AB2O4, wherein the metal element A is Cu, Co or Ni, and the metal element B is Mn, Co, Cr, Al or Fe.
5. The preparation method according to claim 4, characterized in that: The method for preparing the spinel metal oxide comprises the following steps: Mixing a salt of metal element A and a salt of metal element B, a chelating agent, a dispersant and a solvent to obtain a sol solution; Subjecting the sol solution to self-propagating combustion to obtain a metal oxide precursor; calcining the metal oxide precursor to obtain a spinel metal oxide; The molar ratio of the metal element A to the metal element B is 1:
2.
6. The preparation method according to claim 5, characterized in that: The salt of metal element A and the salt of metal element B are independently one or more of nitrate, sulfate, chloride and acetate.
7. The preparation method according to claim 5 or 6, characterized in that: The mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the chelating agent is (1-6):(2-4); the mass ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the dispersant is (1-6):(1-3); the volume ratio of the total mass of the salt of the metal element A and the salt of the metal element B to the solvent is (1-6) g:(20-30) mL.
8. The preparation method according to claim 5, characterized in that: The calcination temperature is 500-900° C. and the calcination time is 2-3 hours.
9. The modified spinel metal oxide prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the modified spinel metal oxide according to claim 9 as an oxygen evolution catalyst in hydrogen production by water electrolysis.
Citation Information
Cited By
Spinel type oxygen evolution electrode and preparation method and application thereof
CN121272453A