Sludge early strength curing agent and preparation method thereof
By using materials such as lithium slag powder and blast furnace slag powder, activators such as Portland cement and hardening accelerators such as salt mud powder, combined with modified polyurethane composite rubber powder as a binder, an early-strength sludge curing agent is prepared, which solves the current problem. There are problems in the technology of high cost, long cycle and low strength of sludge solidification. Rapid hardening and high-strength solidification of sludge are achieved, which promotes the development of sludge resource utilization.
Patent Information
- Application Number
- CN202410837185.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing sludge solidification technology, the cost of cement-based solidification materials is high, the solidification cycle is long, and the strength of the solidified body is low, which limits the promotion and application of silt resource utilization.
It uses lithium slag powder, blast furnace slag powder, calcium silicate slag powder, etc. as the main materials, combined with Portland cement, salt mud powder, etc. as activators and hardening accelerators, and uses modified polyurethane composite rubber powder as the binder to prepare An early strength curing agent for sludge that promotes rapid hardening of sludge and improves the early strength of the solidified body.
It achieves rapid hardening and high-strength solidification of sludge, reduces costs, expands the application prospects of sludge resource utilization, and has industrialization potential.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sludge solidification, and particularly relates to a sludge early strength solidifying agent and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development of urban construction in coastal areas, the number of highways, high-speed railways and other projects has increased. However, due to the great influence of geographical location and climate environment in coastal areas, more and more safety problems of ultra-thick silt soft foundation projects have emerged. At the same time, as my country has increased its management of the water environment, many dredging projects in lakes, rivers, and waterways have produced a large amount of silt. The accumulation of a large amount of silt not only seriously occupies land resources and affects the social environment, but also easily causes secondary disasters such as mudslides. Therefore, the resource utilization of silt has important practical significance for my country's environmental protection.
[0003] Silt solidification is one of the effective ways to utilize silt as a resource. Silt solidification refers to adding an appropriate amount of solidifying materials to the silt, so that the silt has certain mechanical properties through chemical reactions, thereby becoming a soil with a certain bearing capacity. It is used in pile foundation projects, foundation pit support, embankment projects, road projects and fill projects, etc.
[0004] In the prior art, cement-based solidifying materials are usually used for sludge solidification, such as the Chinese patent documents disclosed in publication numbers CN112876184A, CN117776649, and CN111439987A. The cement-based solidifying materials used to solidify sludge in the above documents have the disadvantages of high cost, long solidification cycle, and low strength of the solidified body, which seriously affect the promotion and application of sludge resource utilization.
[0005] Therefore, there is an urgent need to develop a curing agent that can make silt harden quickly, have high strength and low cost, so as to make more efficient resource utilization of silt. Summary of the invention
[0006] The purpose of the present invention is to overcome the above problems existing in the traditional technology and provide a sludge early strength curing agent and a preparation method thereof.
[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0008] The invention provides a sludge early strength curing agent, which comprises 35-93% of a main material, 3-40% of an activator, 2-20% of a hardening accelerator and 2-5% of a modified binder.
[0009] Furthermore, the main material is at least two of lithium slag powder, blast furnace slag powder, and silicon-calcium slag powder.
[0010] Furthermore, the specific surface area of the lithium slag powder is ≥350m 2 / kg;
[0011] The specific surface area of the blast furnace slag powder is ≥350m 2 / kg;
[0012] The specific surface area of the calcium-silicon slag powder is ≥350m 2 / kg.
[0013] Furthermore, the activator is at least one of silicate cement, sulphoaluminate cement, gypsum, potassium sulfate, sodium sulfate, magnesium sulfate, aluminum sulfate, iron sulfate, copper sulfate, calcium oxide, calcium hydroxide, sodium hydroxide, and potassium hydroxide.
[0014] Furthermore, the hardening accelerator is at least one of salt mud powder, domestic waste incineration fly ash powder, magnesium electrolytic slag powder, and magnesium chloride slag powder.
[0015] Furthermore, the specific surface area of the salt mud powder is ≥350m 2 / kg;
[0016] The specific surface area of the fly ash powder from the incineration of domestic waste is ≥350m 2 / kg;
[0017] The specific surface area of the magnesium electrolytic slag powder is ≥350m 2 / kg;
[0018] The specific surface area of the magnesium chloride slag powder is ≥350m 2 / kg.
[0019] Furthermore, the adhesive is prepared by mixing modified polyurethane composite rubber powder, sodium polyacrylate and polyacrylamide in a mass ratio of 1 to 2:1 to 2:1.
[0020] Furthermore, the preparation process of the modified polyurethane composite rubber powder is as follows: polyether amine is added dropwise to polyisocyanate to react, then polyether polyol is added, the temperature is increased to react, and after the reaction is completed, the NCO content in the reaction system is measured to obtain a prepolymer; aminoalkoxysilane is added to the prepolymer to react to obtain a silane-terminated modified polyurethane resin; and the silane-terminated modified polyurethane resin is powdered to obtain a modified polyurethane composite rubber powder.
[0021] The present invention also provides a method for preparing a sludge early strength curing agent, comprising the following steps:
[0022] 1) Weigh the ingredients of the main material according to the proportion, and quickly stir them in a mixer for 3 to 10 minutes to obtain the main material;
[0023] 2) Add the main material prepared in step 1) to the activator, hardening accelerator and modified binder required for the ingredient measurement, and quickly stir for 5 to 20 minutes to prepare the sludge early strength curing agent.
[0024] The present invention also provides an application of a sludge early strength curing agent in sludge curing, and the application steps are as follows:
[0025] 1) Adding a sludge early strength curing agent to the sludge to be cured at 5-100% of the weight of the sludge, adding water and stirring evenly to obtain a sludge slurry; the sludge is marine sludge, lake sludge or river sludge with an organic matter content of ≤20%;
[0026] 2) The sludge slurry is injected into a mold for curing and solidification to obtain a sludge solidified body.
[0027] The beneficial effects of the present invention are:
[0028] 1. In the preparation process of the sludge early strength curing agent, the present invention uses solid wastes such as lithium slag powder, blast furnace slag powder and calcium silicon slag powder as the main materials, and solid wastes such as salt mud powder, domestic waste incineration fly ash powder, magnesium electrolytic slag powder, and magnesium chloride slag powder as hardening accelerators. The present invention has low price and low cost, and can turn waste into treasure, thus having great industrialization prospects.
[0029] 2. The sludge solidifying agent prepared by the present invention is added with a hardening accelerator, which can promote the rapid hardening of the sludge. The sludge solidified body has the characteristics of fast hardening and high early strength, and the sludge can be efficiently utilized as a resource.
[0030] Therefore, the invention has the advantages of wide source of raw materials, low price, simple use process, strong applicability, fast curing, high strength, broad application prospect, etc.
[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] To avoid repetition, the raw materials involved in this specific embodiment are described as follows, and will not be repeated in the examples:
[0034] The main materials are at least two of lithium slag powder, blast furnace slag powder and calcium silicon slag powder. The specific surface area of lithium slag powder is ≥350m 2 / kg; the specific surface area of blast furnace slag powder is ≥350m2 / kg; the specific surface area of calcium silicon slag powder is ≥350m 2 / kg.
[0035] The activator is at least one of silicate cement, sulphoaluminate cement, gypsum, potassium sulfate, sodium sulfate, magnesium sulfate, aluminum sulfate, iron sulfate, copper sulfate, calcium oxide, calcium hydroxide, sodium hydroxide and potassium hydroxide.
[0036] The hardening agent is at least one of salt mud powder, domestic waste incineration fly ash powder, magnesium electrolytic slag powder, and magnesium chloride slag powder. The specific surface area of salt mud powder is ≥350m 2 / kg; the specific surface area of fly ash powder from incineration of domestic waste is ≥350m 2 / kg; the specific surface area of magnesium electrolytic slag powder is ≥350m 2 / kg; the specific surface area of magnesium chloride slag powder is ≥350m 2 / kg.
[0037] The adhesive is prepared by mixing modified polyurethane composite rubber powder, sodium polyacrylate and polyacrylamide in a mass ratio of 1.5:1.5:1. The preparation process of the modified polyurethane composite rubber powder is as follows: 2000 parts of polyetheramine with a molecular weight of 2000 and a functionality of 2 are added dropwise to 500 parts of toluene diisocyanate, the polyetheramine having a molecular weight of 2000 and a functionality of 2, reacting at 40°C for 1 hour, then adding 1600 parts of polyether polyol with a molecular weight of 5000 and a functionality of 3, the molar ratio of NCO groups in toluene diisocyanate to the total active hydrogen in polyether polyol and polyether amine being 2:1, heating to 75°C for reaction for 2 hours, and after the reaction is completed, measuring the NCO content in the reaction system to obtain a prepolymer; adding 700 parts of r-aminopropyltriethoxysilane to the prepolymer, the molar ratio of NCO groups in the prepolymer to active hydrogen in the r-aminopropyltriethoxysilane being 0.95:1, reacting at 45°C in a vacuum environment for 2 hours to obtain a silane-terminated modified polyurethane resin; and powdering the silane-terminated modified polyurethane resin to obtain a modified polyurethane composite rubber powder.
[0038] The relevant specific embodiments of the present invention are as follows:
[0039] Example 1
[0040] This embodiment provides a sludge early strength curing agent, which includes the following components in percentage by weight: 67% of a main material, 20% of an activator, 10% of a hardening accelerator, and 3% of a modified binder.
[0041] The preparation method of the sludge early strength curing agent comprises the following steps:
[0042] 1) According to the composition ratio of the sludge solidifying agent, 10% lithium slag powder and 57% blast furnace slag powder were weighed and rapidly stirred in a mixer for 5 minutes to obtain a main material;
[0043] 2) Add 10% PO 42.5 silicate cement, 10% gypsum, 10% salt mud powder and 3% modified binder to the main material prepared in step 1), and stir rapidly for 5 minutes to prepare the sludge early strength curing agent.
[0044] The early strength curing agent is added to marine silt with an organic matter content of 4.2% at a ratio of 12% by weight of the silt, and an appropriate amount of water is added and stirred evenly to obtain a slurry with a solid content of 65%. The slurry is injected into a mold and cured for 28 days to obtain a solidified body with a compressive strength of 4.2 MPa.
[0045] Example 2
[0046] This embodiment provides a sludge early strength curing agent including the following components in percentage by weight: 67% of a main material, 25% of an activator, 5% of a hardening accelerator, and 3% of a modified binder.
[0047] The preparation method of the sludge early strength curing agent comprises the following steps:
[0048] 1) According to the composition ratio of the sludge solidifying agent, 55% of blast furnace slag powder and 12% of calcium silicon slag powder were weighed and rapidly stirred in a mixer for 5 minutes to obtain a main material;
[0049] 2) Add 15% sulphoaluminate cement, 10% calcium oxide, 5% magnesium chloride slag powder and 3% modified binder to the main material prepared in step 1), and stir rapidly for 5 minutes to prepare the sludge early strength curing agent.
[0050] The early strength curing agent is added to the lake silt with an organic matter content of 8.5% at 10% of the silt weight, stirred and adjusted to obtain a silt slurry with a solid content of 55%, and injected into a mold for standard curing for 28 days to obtain a solidified body with a compressive strength of 1.1 MPa.
[0051] Example 3
[0052] This embodiment provides a sludge early strength curing agent, which includes the following components in percentage by mass: 82% of a main material, 10% of an activator, 5% of a hardening accelerator, and 3% of a modified binder.
[0053] The preparation method of the sludge early strength curing agent comprises the following steps:
[0054] 1) According to the composition ratio of the sludge solidifying agent, 50% of blast furnace slag powder and 17% of calcium silicon slag powder were weighed and rapidly stirred in a mixer for 5 minutes to obtain a main material;
[0055] 2) Add 15% sulphoaluminate cement, 5% potassium sulfate, 5% calcium oxide, 5% domestic waste incineration fly ash powder and 3% modified binder to the main material prepared in step 1), and stir rapidly for 8 minutes to prepare the sludge early strength curing agent.
[0056] The early strength curing agent was added to river silt with an organic matter content of 12.5% at a ratio of 12% by weight of the silt, stirred and adjusted to obtain a silt slurry with a solid content of 40%, and injected into a mold for standard curing for 28 days to obtain a solidified body with a compressive strength of 0.9 MPa.
[0057] Example 4
[0058] This embodiment provides a sludge early strength curing agent including the following components in percentage by weight: 52% of a main material, 35% of an activator, 10% of a hardening accelerator, and 3% of a modified binder.
[0059] The sludge early strength curing agent comprises the following steps:
[0060] 1) According to the composition ratio of the sludge solidifying agent, 15% of lithium slag powder, 30% of blast furnace slag powder and 7% of calcium silicon slag powder were weighed and rapidly stirred in a mixer for 10 minutes to obtain a main material;
[0061] 2) Add 10% gypsum, 5% magnesium sulfate, 10% calcium oxide, 5% magnesium electrolytic slag powder, 5% live garbage incineration fly ash powder and 3% modified binder to the main material prepared in step 1), and stir rapidly for 10 minutes to prepare the sludge early strength curing agent.
[0062] The early strength curing agent is added to marine sludge with an organic matter content of 7.5% at 8% of the sludge weight, stirred and adjusted to obtain a sludge slurry with a solid content of 50%, and injected into a mold for standard curing for 28 days to obtain a solidified body with a compressive strength of 2.2 MPa.
[0063] Example 5
[0064] This embodiment provides a sludge early strength curing agent, which includes the following components in percentage by weight: 47% of a main material, 40% of an activator, 10% of a hardening accelerator, and 3% of a modified binder.
[0065] The preparation method of the sludge early strength curing agent comprises the following steps:
[0066] 1) According to the composition ratio of the sludge solidifying agent, 5% of lithium slag powder and 42% of silicon-calcium slag powder were weighed and rapidly stirred in a mixer for 10 minutes to obtain a main material;
[0067] 2) Add 20% PO 42.5 silicate cement, 15% gypsum, 5% sodium hydroxide, 5% salt mud powder, 5% magnesium chloride slag powder and 3% modified binder to the main material prepared in step 1), and stir rapidly for 15 minutes to prepare the sludge early strength curing agent.
[0068] The early strength curing agent is added to the lake silt with an organic matter content of 5.6% at a ratio of 15% by weight of the silt, stirred and adjusted to obtain a silt slurry with a solid content of 60%, and injected into a mold for standard curing for 28 days to obtain a solidified body with a compressive strength of 1.9 MPa.
[0069] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A sludge early strength curing agent, characterized in that: It comprises 35-93% of main material, 3-40% of activator, 2-20% of hardening accelerator and 2-5% of modified binder.
2. The sludge early strength curing agent according to claim 1, characterized in that: The main materials are at least two of lithium slag powder, blast furnace slag powder and silicon-calcium slag powder.
3. The sludge early strength curing agent according to claim 2, characterized in that: The specific surface area of the lithium slag powder is ≥350m 2 / kg; The specific surface area of the blast furnace slag powder is ≥350m 2 / kg; The specific surface area of the calcium-silicon slag powder is ≥350m 2 / kg.
4. The sludge early strength curing agent according to claim 1, characterized in that: The activator is at least one of silicate cement, sulphoaluminate cement, gypsum, potassium sulfate, sodium sulfate, magnesium sulfate, aluminum sulfate, iron sulfate, copper sulfate, calcium oxide, calcium hydroxide, sodium hydroxide and potassium hydroxide.
5. The sludge early strength curing agent according to claim 1, characterized in that: The hardening accelerator is at least one of salt mud powder, domestic waste incineration fly ash powder, magnesium electrolytic slag powder, and magnesium chloride slag powder.
6. The sludge early strength curing agent according to claim 5, characterized in that: The specific surface area of the salt mud powder is ≥350m 2 / kg; The specific surface area of the fly ash powder from the incineration of domestic waste is ≥350m 2 / kg; The specific surface area of the magnesium electrolytic slag powder is ≥350m 2 / kg; The specific surface area of the magnesium chloride slag powder is ≥350m 2 / kg.
7. The sludge early strength curing agent according to claim 1, characterized in that: The adhesive is prepared by mixing modified polyurethane composite rubber powder, sodium polyacrylate and polyacrylamide in a mass ratio of 1 to 2:1 to 2:
1.
8. The sludge early strength curing agent according to claim 7, characterized in that: The preparation process of the modified polyurethane composite rubber powder is as follows: polyether amine is added dropwise to polyisocyanate to react, then polyether polyol is added, the temperature is increased to react, and after the reaction is completed, the content of NCO in the reaction system is measured to obtain a prepolymer; aminoalkoxysilane is added to the prepolymer to react to obtain a silane-terminated modified polyurethane resin; and the silane-terminated modified polyurethane resin is powdered to obtain the modified polyurethane composite rubber powder.
9. The method for preparing the sludge early strength curing agent according to any one of claims 1 to 8, characterized in that: The steps include: 1) Weigh the ingredients of the main material according to the proportion, and quickly stir them in a mixer for 3 to 10 minutes to obtain the main material; 2) Add the main material prepared in step 1) to the activator, hardening accelerator and modified binder required for the ingredient measurement, and quickly stir for 5 to 20 minutes to prepare the sludge early strength curing agent.
10. Use of the sludge early strength curing agent according to any one of claims 1 to 8 in sludge curing, characterized in that: The application steps are as follows: 1) Adding a sludge early strength curing agent to the sludge to be cured at 5-100% of the weight of the sludge, adding water and stirring evenly to obtain a sludge slurry; the sludge is marine sludge, lake sludge or river sludge with an organic matter content of ≤20%; 2) The sludge slurry is injected into a mold for curing and solidification to obtain a sludge solidified body.