Ceramic clay formula capable of improving drying strength of green body
By using a specific proportion of mud and clinker in the clay formula, as well as fructose fiber as a reinforcing agent, the problem of cracking during the drying process of the green pottery is solved, the drying strength and yield are improved, and the firing performance and performance of the pottery are ensured. cost control.
Patent Information
- Application Number
- CN202411010615.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
AI Technical Summary
Pottery green bodies tend to shrink unevenly during the drying and dehydration process, causing surface cracks and cracks, affecting the yield of finished products.
A clay formula is used, including slime and clinker. The composition of the slime is 55-70% silicon oxide, 16-25% alumina, 3-5% sodium potassium salt, and the remainder is iron oxide, titanium oxide and burnable The mass ratio of clinker to slime is 1:8-10. Fructose fiber is added as a reinforcing agent. The particle size distribution is above 250 mesh to improve the drying strength of the green body.
It effectively improves the drying strength of the green body, reduces the risk of cracking, improves the yield, and ensures the firing temperature and performance while controlling costs.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, relates to raw materials for ceramic production, and specifically relates to a pottery clay formula capable of improving the drying strength of a green body. Background Art
[0002] Pottery clay is clay used to make pottery. It refers to clay that contains minerals and has yellow-brown, gray-white, red-purple and other colors, and has good plasticity. The mineral components are mainly montmorillonite and kaolin, containing silicon oxide, aluminum oxide and other metal oxides, as well as considerable water and organic matter that can be burned.
[0003] In the process of making pottery, it is necessary to first shape the green body. After the green body is naturally dried or dried for dehydration, it enters the kiln to fire the pottery at high temperature. During the dehydration process, as the water evaporates, the green body tends to shrink unevenly, causing cracks to form on the surface of the green body. Summary of the invention
[0004] In view of the defects of the prior art mentioned above, the present invention discloses a clay formula which can improve the drying strength of the green body.
[0005] The present invention comprises ore mud and clinker, wherein the contents of the components in the ore mud are 55-70% silicon oxide, 16-25% aluminum oxide, 3-5% sodium potassium salt, and the remainder are iron oxide, titanium oxide and burnable materials; the clinker is a material obtained by firing the ore mud, and the mass ratio of the clinker to the ore mud is 1:8-10, wherein the particle size distribution of the ore mud and the clinker is 70-75wt% and is above 250 mesh.
[0006] Preferably, the clay formula contains a reinforcing agent, the reinforcing agent contains fructose fiber, and the mass proportion of the fructose fiber in the clay formula is 0.2-0.5%.
[0007] Specifically, the enhancer is a fructose fiber composite additive.
[0008] Specifically, it contains 0-10% iron oxide and 0-2% titanium oxide.
[0009] The invention adopts an improved clay formula capable of improving the drying strength of green bodies, thereby controlling the processing cost and improving the drying strength, so that the green bodies are not easy to crack during the drying and dehydration process, thereby improving the yield rate of green bodies. DETAILED DESCRIPTION
[0010] In order to more intuitively and clearly describe the specific details of the technical solution of the present invention, a detailed description will be given below in conjunction with specific embodiments.
[0011] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely explained below in combination with the specific implementation methods of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0012] The pottery clay formula of the present invention comprises ore mud and clinker, wherein the contents of the components in the ore mud are 55-70% silicon oxide, 16-25% aluminum oxide, 0-10% iron oxide, 0-2% titanium oxide, 3-5% sodium potassium salt, and the remainder is burnable material; the clinker is a material obtained by firing the ore mud, and the mass ratio of the clinker to the ore mud is 1:8-10, wherein the particle size distribution of the ore mud and the clinker is 70-75wt% below 250 mesh.
[0013] Mineral mud is a layer of soil obtained directly from nature. The content of various components in the mineral mud varies with the geographical location of the mine and the depth of soil excavation. In order to obtain a suitable ratio of each component, it can be obtained by digging mineral mud from different layers in different mines and mixing them in a certain proportion.
[0014] For example, the applicant can obtain the above-mentioned mineral mud by taking soil from the second layer of pit No. 1, the sixth layer of pit No. 1, and the second layer of pit No. 2 in a mass ratio of 1:1:1 at the clay mine in Laimou Town, Rong County, Zigong City, Sichuan Province. In other mines, after measuring the content of the main components of each layer, the above-mentioned mineral mud can also be obtained by mixing different types of mineral mud.
[0015] Most of the burnable materials are organic matter and water, and there are also a small amount of minerals that decompose under high temperatures.
[0016] By using a ratio of 55-70% silicon oxide and 16-25% aluminum oxide, a firing temperature of about 1200 degrees Celsius can be obtained. The firing temperature refers to the temperature required for the ceramic blank to be sintered into an object. When the firing temperature reaches 1200 degrees Celsius, porcelain can be obtained and a high-temperature glaze layer of suitable temperature can be fired at the same time. Alumina is combined with sodium potassium salt at this temperature. Sodium potassium salt acts as a flux to completely melt the aluminum oxide. The content of sodium potassium salt as a flux should not be too high, otherwise it will easily cause deformation of the blank during the firing process.
[0017] The fired ceramic crystals contain mullite phase, glass phase and free quartz phase, among which the mullite phase content can significantly improve the extreme cold and hot properties of the ceramic. Only when the firing temperature is above 1200 degrees Celsius can the proportion of mullite phase reach more than 30%, thus obtaining a ceramic body with good extreme cold and hot properties.
[0018] 0-10% iron oxide, 0-2% titanium oxide and burnable materials are the inevitable components in naturally formed mineral mud. The inventor did not deliberately seek to adjust the ratio of these three components in the clay mixing ratio.
[0019] The finer the particle size, the easier it is to form a water film on the particle surface, which improves the plasticity of the clay and makes it less likely to crack. However, the finer the particle size, the greater the risk of shrinkage during drying and firing. According to the applicant's experiment, it can be seen that when the particle size is below 250 mesh and is more than 70%, the dry strength reaches 3.96, and the maximum increase after three days of aging is 4.65. The percentage increase after three days of aging is the largest and the absolute value is the highest.
[0020]
[0021] The dry strength of the green body obtained after adding the clinker is tested after aging as shown in the following table. Aging means keeping the wet mud moist for 3 days, and the internal organic matter will naturally decompose. During the aging process, the moisture of the mud will be more uniform, the mineral moisture absorption and expansion process will be basically completed, the internal stress release will be basically finished, the water film between the particles will be basically uniform, and the ion exchange will be basically completed, so it will be more stable after being put into use. This will improve the strength of the green body and effectively reduce the cracking of the wet body.
[0022]
[0023] Among them, the reinforcing agent can be a fructose fiber composite additive. The function of fructose fiber is to connect the particles to form a long chain, which reduces the cracking of the wet blank during the drying process of the wet blank. The fructose fiber used as a reinforcing agent will be completely burned during the burning process, and will not affect the ablation molding. The reinforcing agent is preferably a fructose fiber composite additive, which contains about 60% natural fructose fiber and has low cost.
[0024] In the absence of enhancer, it can be seen that before the clinker content reaches 10%, the various parameters increase significantly with the increase of clinker percentage, and after exceeding 10%, the various parameters no longer increase.
[0025] After adding the reinforcing agent, the failure load, fracture thickness and flexural strength of the 10% clinker increased significantly.
[0026] After adding clinker with a certain particle size, since the clinker has been burned out, there is no drying shrinkage and firing shrinkage during the second sintering, so the overall shrinkage is reduced to reduce the risk. In addition, the clinker particles are selected with the best particle size ratio to add raw materials to play the role of aggregate and improve the stress resistance of the formed body. During the sintering process, the mullite phase of the clinker mineral composition has been formed, thereby improving the extreme cold and heat resistance and facilitating the firing control. The defective product test of the product with and without clinker is shown in the following table.
[0027]
[0028] The experimental products in the table are manufactured at the same workstation and fired in batches at the same time. After firing, the products are tested for a certain degree of vacuum and negative pressure air tightness, and the pressure holding time is not less than 3 minutes to test the leakage test.
[0029] The foregoing describes various preferred embodiments of the present invention. Unless the preferred implementation modes in various preferred embodiments are obviously self-contradictory or based on a certain preferred implementation mode, various preferred implementation modes can be arbitrarily superimposed and used in combination. The embodiments and specific parameters in the embodiments are only for clearly describing the invention verification process of the inventor, and are not used to limit the patent protection scope of the present invention. The patent protection scope of the present invention shall still be based on its claims. All equivalent structural changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.
Claims
1. A clay formula for improving the dry strength of a green body, characterized in that: It includes ore mud and clinker, wherein the contents of various components in the ore mud are 55-70% silicon oxide, 16-25% aluminum oxide, 3-5% sodium potassium salt, and the rest are iron oxide, titanium oxide and burnable materials; the clinker is the material obtained by firing the ore mud, the mass ratio of the clinker to the ore mud is 1:8-10, wherein the particle size distribution of the ore mud and the clinker is 70-75wt% and is above 250 mesh.
2. The clay formula according to claim 1, characterized in that: The clay formula contains a reinforcing agent, and the reinforcing agent contains fructose fiber. The mass proportion of the fructose fiber in the clay formula is 0.2-0.5%.
3. The clay formula according to claim 1, characterized in that: The reinforcing agent is a fructose fiber composite additive.
4. The clay formula according to claim 1, characterized in that: Contains 0-10% iron oxide and 0-2% titanium oxide.
Citation Information
Patent Citations
Ceramic liner bricks for electrothermal - storage furnaces
CH542158A
Preparation process of transmuted tile with uniform transmutation effect
CN107827432A
Ceramic large statue forming process
CN115042296A
Cited By
Easily demoulded pottery jar preparation process
CN120170869A
Process for preparing a demouldable ceramic jar
CN120170869B