Preparation and application of novel environment-friendly nano hybrid solid lubricant additive
By combining modified polymethylsilsesquioxane nanoparticles and hydrosilylation products with borax and silicone oil, an environmentally friendly nanohybrid solid lubricant additive with high thermal stability and low friction coefficient is prepared, which solves the problem of solid lubricant additives in the existing technology. Better friction reduction performance is achieved amid issues of poor thermal stability and environmental health threats under high temperature and pressure conditions.
Patent Information
- Application Number
- CN202410762191.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing solid lubricating additives have poor thermal stability under high temperature and high pressure conditions, pose potential threats to the environment and health, and are difficult to effectively reduce friction.
It uses modified polymethylsilsesquioxane nanoparticles and hydrosilylation products, combined with borax and silicone oil, to prepare high thermal stability, low friction coefficient and high wear resistance through esterification, hydrosilylation and ultrasonic dispersion processes. Environmentally friendly nanohybrid solid lubricant additive.
Significantly improves the thermal stability and friction reduction performance of lubricating additives, reduces friction, is suitable for high temperature and high pressure scenarios, and at the same time improves environmental sustainability and safety.
Smart Images

Figure CN118772192A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of additive technology application, and in particular to the preparation and application of a novel environmentally friendly nano hybrid solid lubricating additive. Background Art
[0002] From everyday household items to medium and heavy-duty industries, the use of lubricants is as important as fuel. Friction is an inherent force in nature that is useful in some situations, but in other cases, reducing friction is essential for the smooth and uninterrupted operation of mechanical components. When friction reduction is required, the application of lubricants and lubricant additives plays a key role in minimizing wear, reducing power consumption and reducing energy losses. Solving friction problems involves using a variety of lubricants in different physical states, including liquids and solids, to meet specific needs and requirements. Liquid lubricants are suitable for systems that operate at lower temperatures and pressures, while solid lubricants are suitable for systems that generate high temperatures and are subject to high pressures on the friction surfaces. Solid lubricants are an important category that includes metal-containing and non-metal-containing compounds, and both types are suitable for different friction systems.
[0003] The expansion of manufacturing and industrial operations has had a negative impact on air quality and the environment. Biological and environmental sustainability are threatened by the high energy consumption associated with high friction in automotive and industry, which highlights the importance of eco-tribology. Current initiatives focus on replacing polluting lubricant additives with bio-based materials to mitigate these environmental issues.
[0004] Silicone oil (SO) is widely used in medical and cosmetic fields due to its acclaimed biosafety and adaptability. With reasonable market price, thermal stability and excellent dielectric properties, it has the potential to enhance performance and reduce friction in eco-tribology applications with further improvements.
[0005] In order to solve the harmful effects of solid lubricant additives and improve their thermal stability, this patent aims to design an environmentally friendly, heat-resistant and safe solid lubricant for industry workers and everyday consumers. We have adopted commonly used borax and highly stable new silsesquioxane-based materials.
[0006] Borates such as borax and boric acid are common lubricating additives in various liquids, known for their low coefficient of friction, high wear resistance and high compatibility with friction interfaces. Borax (Na2B4O7) in the form of pentahydrate (Na2B4O7·5H2O) and decahydrate (Na2B4O7·10H2O) is widely used in metal drawing, enamel, flux, textiles, cosmetics and soap industries.
[0007] Silsesquioxane is an important member of the family of silicon-containing compounds with a three-dimensional Si-O-Si network, which makes this material a good choice for achieving the desired properties with high thermal stability. To obtain these properties, novel nano-polymethylsilsesquioxane hybrid particles containing long carbon chains with narrow size distribution were prepared. These types of materials are used to reduce friction due to their low surface energy, environmental friendliness and lubricating effect of long carbon or alkyl chains.
[0008] Silicone oil (SO) is of great value due to its biosafety and adaptability and is widely used in the medical and cosmetic fields. With its reasonable market price and good thermal stability, it also has the potential to reduce friction in eco-tribological applications through further improvements. In the study of silicone oil lubrication, different types of materials of this type have been prepared, for example, the fluorinated octadecylamine salt of decaprylfluorooctanoic acid was added to silicone oil to enhance the friction properties, thereby significantly improving the wear and friction reduction performance. Chlorophenyl-substituted silicone oil and trifluoropropyl siloxane were prepared, and trifluoropropyl silicone oil became a top-level load-bearing oil with high anti-wear properties. Meanwhile, lanthanum metal-based LaF3 nanoparticles modified with fluorosilane enhanced the friction properties of fluorosilicone oil as a solid lubricant additive. The surface-modified LaF3 nanoparticles significantly improved the friction coefficient and wear resistance. However, their disadvantages include low thermal stability and potential health hazards. Therefore, the lubricating additive modified with borax (Na2B4O7) effectively solves the shortcomings of its poor thermal stability and inability to be applied in high temperature and high pressure scenarios, and obtains a new type of environmentally friendly nano-hybrid solid lubricating additive with the characteristics of low friction coefficient, high wear resistance and good compatibility with the friction interface. Summary of the invention
[0009] In view of the deficiencies of the prior art, the present invention prepares an environmentally friendly lubricating additive with high thermal stability, good friction reduction performance and good wear resistance to silicone oil (polydimethylsiloxane).
[0010] In order to achieve the above objectives, the present invention provides a method for preparing an environmentally friendly nano-hybrid solid lubricant additive, comprising the following steps:
[0011] Preferably, polymethylsilsesquioxane nanoparticles (P-NP) are prepared by adding 10-50 g of methyltriethoxysilane (MTES) to water containing 0.1-10 g of sodium dodecylbenzene sulfonate (SDBS) at a stirring speed of 150-750 rpm for 10-100 minutes.
[0012] Preferably, the reaction is catalyzed by 0.1-10 mL NH4OH (2-40% v / v) and lasts for 1-10 h at 10-100° C. Finally, the P-NPs are separated from the solvent mixture by centrifugation and washed with distilled water three to five times, thereby obtaining a white material.
[0013] Preferably, the above white material is dried in a vacuum oven at 10-100° C. for 2-24 hours, and it shows a bright white powder appearance, and is further ground into fine particles using a ball mill.
[0014] Preferably, oleic acid or octadec-9-enoic acid is added into a three-necked flask connected to a glass water separator and a condenser to carry out the esterification reaction.
[0015] Preferably, the above reaction is stirred continuously at 10-100°C and 100-500 rpm. The molar ratio of oleic acid to ethanol is 1:1, 1:2, 1:3, 1:4, 1:5, and the amount of sulfuric acid used as a catalyst is 0.1-1.0 g (purity 90-99%). While heating the reaction mixture, the evaporated ethanol is collected in a laboratory glass water separator after cooling, and the total reaction time is 1-24 hours.
[0016] Preferably, the resulting ethyl 9-octadecenoate or ethyl oleate (EO) is washed in a separatory funnel to remove H2SO4, and the excess H2SO4 is titrated with KOH, and the EO is purified by rotary evaporation to remove any unreacted material.
[0017] Preferably, the hydrosilylation reaction is carried out in an inert environment of N2 gas by taking 1-10 g of ethyl oleate EO in 10-100 mL of toluene solvent and keeping mixing at a stirring speed of 100-500 rpm.
[0018] Preferably, triethoxysilane (TES) is slowly added using a micromelt pump and the addition is completed within 1-24 hours, and the molar ratio of EO to TES is 1:1, 1:2, 1:3, 1:4, 1:5.
[0019] Preferably, chloroplatinic acid H2PtCl6 (0.01-0.1wt% in isopropanol) is used in a flask, the maximum concentration is 60ppm, the reaction temperature is 10-100°C, the reaction time is 1-96h, and the unreacted compounds are separated by a rotary evaporator. Relative to the amount of all reactants used, 80-90% of the hydrosilylation product is obtained.
[0020] In FTIR, the main characteristic peak of the hydrosilylation product is at 1622 cm -1 The C=C of the olefin in the absence of ethyl oleate (EO) at 1025 cm -1 (bend) and 1120cm -1 There is a Si-O bond at 760 cm -1 The presence of Si-C (stretching) at the 200 nm region confirms the successful hydrosilylation of triethoxysilane (TES) with EO, as shown in Figure 5. Figure 1shown.
[0021] Preferably, P-NPs are modified with ethyl 11-(triethoxysilyl)undecanoate (S2EO) by ultrasonically dispersing P-NPs (2-5 g) and 0.1-1 g S2EO in a solution of 100-300 mL of water (20-130 mL) and ethanol (80-170 mL) at 10-100° C. for 1-10 minutes.
[0022] Preferably, the mixture is added to a 50-500 mL three-necked flask for premixing, with a stirring speed of up to 100-500 rpm and a stirring time of 10-300 minutes.
[0023] Preferably, the solution pH is maintained at 7.5-9.5 by slow addition of ammonium hydroxide (20-50% v / v).
[0024] Preferably, a 0.1-1 mol / L methylamine solution prepared in 5-250 mL of deionized water is added dropwise to the above solution, and the mixture is stirred and heated at 10-100° C. for a reaction of 1-24 hours.
[0025] Preferably, after the above reaction is completed, it is cooled to room temperature, and the mixture is subjected to high-speed centrifugation, and washed with ethanol and water for multiple cycles to make the mixture neutral, and the obtained white product of S2EO-modified P-NPs is dried in a hot air vacuum at 10-100°C for 1-24 hours.
[0026] Compared with the prior art, this application has the following beneficial effects:
[0027] The present invention is based on modified nanoparticles of polymethylsilsesquioxane (PMSQ), adopts environmentally friendly materials, has high thermal stability, good friction reduction performance and wear resistance (friction performance) to silicone oil (polydimethylsiloxane). BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is the FTIR Fourier transform infrared spectra of 9-(triethoxysilyl) ethyl octadecanoate (S2EO), ethyl oleate (EO), and triethoxysilane (TES);
[0029] Figure 2 are the FTIR Fourier transform infrared spectra of P-NPs, S2EO and P-NPs-S2EO;
[0030] Figure 3 are SEM images of P-NPs (a) and P-NPs-S2EO (b);
[0031] Figure 4are EDS spectra of P-NPs with low (a) and P-NPs-S2EO with high carbon and oxygen contents (b);
[0032] Figure 5 are the TGA curves of borax (a), P-NPs (b), and P-NPs-S2EO (c);
[0033] Figure 6 is a comparison chart of the average COF values of the sample mixtures containing silicone oil + borax, silicone oil + P-NPs, and siloxane + P-NPs-S2EO with different weight ratios of 0 (a), 0.2 (b), 0.3 (c), 0.4 (d), and 0.5 (e). DETAILED DESCRIPTION
[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in the present application belong to the scope of protection of this application.
[0035] Example 1
[0036] Polymethylsilsesquioxane nanoparticles (P-NPs) were prepared by adding 24 g of methyltriethoxysilane (MTES) to 270 mL of water containing 0.7 g of sodium dodecylbenzene sulfonate (SDBS) at a stirring speed of 750 rpm for 40 minutes. The reaction was catalyzed by 0.5 mL of NH4OH (28% v / v) and continued for 10 h at 30 ° C. Finally, P-NPs were separated from the solvent mixture by centrifugation and washed three times with distilled water. A white material was thus obtained, which was dried in a vacuum oven at 70 ° C for 8 hours and further ground into fine particles with a ball mill. Oleic acid or octadecene-9-enoic acid was added to a 250 mL three-necked flask connected to a laboratory glass water separator and a condenser, and the reaction was continued at 50 ° C and 250 rpm. The molar ratio of oleic acid to ethanol was 1:5, and the amount of sulfuric acid used as a catalyst was 0.3 g (purity 98%). While heating the reaction mixture, the ethanol evaporated after cooling was collected in a laboratory glass water separator. Since the esterification reaction is reversible, it is necessary to maintain the optimal amount of reactants in order to keep the reaction in the forward direction. Therefore, the collected ethanol is fed back to the flask. The total reaction time is 5 hours. Afterwards, the resulting 9-octadecenoic acid ethyl ester or ethyl oleate (EO) is washed in a separatory funnel to remove H2SO4, and the excess H2SO4 is titrated with KOH. Finally, EO is purified by a rotary evaporator to remove any unreacted material.
[0037] In an inert environment of N2 gas, 3.1g of ethyl oleate EO was taken in 60mL toluene solvent and kept mixed at a stirring speed of 500rpm for hydrosilylation. Then, triethoxysilane (TES) was slowly added with a micromelt pump and the addition was completed within 12 hours, with a molar ratio of EO to TES of 1:3. Chloroplatinic acid H2PtCl6 (0.08wt% in isopropanol) was used in a flask, with a maximum concentration of 60ppm, and a reaction temperature of 70°C throughout the process. After 48 hours, the reaction was completed and the unreacted compounds were separated by a rotary evaporator. Relative to the amount of all reactants used, 81% of the hydrosilylation product was obtained. Finally, yellow viscous liquid 9-(triethoxysilyl) ethyl octadecanoate appeared as a product. For simplicity, the hydrosilylation product of EO, i.e. 9-(triethoxysilyl) ethyl octadecanoate. The formation of the product can be confirmed by FTIR Fourier transform infrared spectrogram.
[0038] like Figure 1 As shown, the main characteristic peak of the hydrosilylation product is at 1622 cm -1 The C=C of the olefin in the absence of ethyl oleate (EO) at 1025 cm -1 (bend) and 1120cm -1 There is a Si-O bond at 760 cm -1 The presence of Si-C (stretching) at 40° confirmed the successful hydrosilylation of triethoxysilane (TES) with EO.
[0039] P-NPs were modified with 11-(triethoxysilyl)undecanoic acid ethyl ester (S2EO) by ultrasonically dispersing P-NPs (2.5 g) and 0.3 g S2EO in 100 mL of water (30 mL) and ethanol (70 mL) solution at 40°C for 30 min. The mixture was then premixed before adding any new material in a 250 mL three-necked flask for 30 min with stirring speed up to 400 rpm. pH 9.5 was carefully maintained and frequently monitored by slowly adding ammonium hydroxide (28% v / v). A 0.2 mol% methylamine solution prepared separately in 25 mL of deionized water was added dropwise while heating the reaction at 70°C with continuous stirring for 4 h. After the reaction was completed, it was cooled to room temperature and the sludge was centrifuged at high speed and washed with ethanol and water for multiple cycles to make the mixture neutral. Finally, the white product of S2EO-modified P-NPs was dried in a hot air vacuum at 70°C for 6 h. We abbreviate this modified product as P-NPs-S2EO. FTIR, SEM and EDS confirmed this modification.
[0040] like Figure 2 As shown, in P-NP, the Si-O-Si bond appears at 1120 cm -1(Stretched) and 1025cm -1 (bending), while the CH (stretching) frequency for all three materials appears at 2950 cm -1 , while Si-C (stretching) appears at 760 cm -1 The CH signal of Si-CH3 also appears at 1260 cm -1 More importantly, in P-NPs-S2EO, the carbonyl carbon of the ester group appears at 1730 cm -1 This clearly indicates that the long carbon chains containing ester groups have been successfully attached to the surface of P-NPs. For the comparison of unmodified particles P-NPs and modified P-NPs-S2EO, it can be seen that Figure 3 The confirmation of P-NP modification can be achieved by observing the change in the percentage content of the basic elements. Figure 4 The EDS data in Figure 3 show that the weight percentages of carbon and oxygen (C = 18.8 wt% and O = 21.1 wt%) were low before modification. However, after modification with S2EO, the percentages of carbon and oxygen (C = 44.2 wt% O = 49.4 wt%) increased, demonstrating the effect of S2EO on the surface of P-NPs-S2EO.
[0041] The thermal properties of borax, P-NPs, and P-NPs-S2EO were analyzed using a TGA machine in an air atmosphere up to 800°C. The W100 (weight loss at 100°C) of borax and P-NPs were 24.1% and 0.5%, respectively, while the W200 (weight loss at 200°C) was 34.3% and 2.6%. In contrast, P-NPs-S2EO showed a weight loss of 0.6% and 1.8% at the respective temperatures, which was much lower than that of borax, as shown in Figure 2. Figure 5 This indicates that the modified nanoparticles have high thermal properties.
[0042] In this regard, P-NPs-S2EO is 32.5% more thermally stable than borax at W200, a fact that can be seen from the summarized values in Table 1:
[0043] Table 1 TGA data of borax, P-NPs and P-NPs-S2EO
[0044]
[0045] Example 2
[0046] The difference between this embodiment and embodiment 1 is that the tribological properties of SO will be examined by incorporating borax, P-NPs designed by us and P-NPs-S2EO as solid lubricant additives into SO (base oil). In order to study the tribological properties of lubricating materials, we used a tribometer called MICROTEST MT / 60 Pin-on-Disk tester, which is connected to a speed controller (NT4002) through a motor drive and a computer servo control suitable for testing. For each test of each sample, a new iron container is used. The iron container is properly fixed to the disc of the machine with a hinge, and then the test sample is poured into the container. In order to ensure the consistency of all tests, each sample and iron container are treated equally. The iron container and the tip of the pin are carefully cleaned and polished to form a smooth surface for accurate testing.
[0047] Borax, P-NPs, and P-NPs-S2EO were dispersed in SO. To improve particle dispersion, each sample mixture was sonicated and mechanically stirred at 40 °C for 30 min to achieve homogeneity. All these sampling parameters are summarized in Table 2.
[0048] Table 2 Sample test parameters
[0049]
[0050] 0.2 wt% P-NPs-S2EO (COF=0.008) in silicone oil reduced friction by 93.23% compared to 0 wt%. The average COF values of sample mixtures of silicone oil + different concentrations of borax and P-NPs-S2EO were compared to each other. The comparison showed that P-NPs-S2EO (COF=0.008) reduced friction by 50.51% even at low concentrations (0.2 wt%) compared to 0.4 wt% borax (COF=0.067). A huge difference was observed when P-NPs-S2EO (COF=0.008) reduced friction by 65.26% at 0.2 wt%, compared to its unmodified form P-NPs (COF=0.085) at 0.3 wt%. Comparison of the COF reduction performance of borax, P-NPs and P-NPs-S2EO is shown in Figure 2. Figure 6 The combined graph provides a simple way to understand the maximum reduction of COF, which shows that P-NPs-S2EO (maximum COF reduction = 93.23%) performs better than borax (maximum COF = 42.7%), and borax performs better than P-NPs (maximum COF reduction = 27.97). Table 3 analyzes the improvement performance of all lubricants in terms of friction reduction:
[0051] Table 3 Comparison of friction properties of all lubricants
[0052]
[0053] a The largest percentage reduction in COF of all lubricants compared to the COF value of 0.118 for pure silicone oil
[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Without departing from the principle of the present invention, modifications and improvements to the technical solutions described in the above specific embodiments are deemed to be within the protection scope of the present invention.
Claims
1. Preparation and application of a new environmentally friendly nano hybrid solid lubricant additive, characterized in that: Hydrosilylation of ethyl oleate with triethoxysilane forms ethyl 11-(triethoxysilyl)undecanoate.
2. The environmentally friendly nano hybrid solid lubricant additive according to claim 1, characterized in that: In the hydrosilylation reaction, the molar ratio of ethyl oleate to triethoxysilane is 1:1, 1:2, 1:3, 1:4, 1:
5.
3. The environmentally friendly nano hybrid solid lubricant additive according to claim 2, characterized in that: The hydrosilylation process was carried out at a temperature of 70°C for 24-72 hours.
4. The environmentally friendly nano hybrid solid lubricant additive according to claim 3, characterized in that: Polymethylsilsesquioxane nanoparticles (P-NPs) were modified with 11-(triethoxysilyl) undecenoic acid ethyl ester (S2EO) as raw material to prepare P-NPs-modified S2EO nanolubricating additive, named P-NPs-S2EO.
5. The environmentally friendly nano hybrid solid lubricant additive according to claim 4, characterized in that: During the modification of polymethylsilsesquioxane nanoparticles (P-NPs) with 11-(triethoxysilyl) undecanoate (S2EO), the stirring speed was maintained at 400 rpm.
6. The environmentally friendly nano hybrid solid lubricant additive according to claim 5, characterized in that: During the modification of polymethylsilsesquioxane nanoparticles (P-NPs) with 11-(triethoxysilyl) undecanoate (S2EO), the solution pH was maintained at 7.7-9.5 by slowly adding ammonium hydroxide (28% v / v).
7. The environmentally friendly nano hybrid solid lubricant additive according to claim 6, characterized in that: In order to improve the friction performance of silicone oil (10 g test amount), 0.2 wt % P-NPs-S2EO was added to the silicone oil, and the friction ratio was reduced to 93.