Polypeptide for preparing hydrogel, polypeptide hydrogel as well as preparation method and application of polypeptide hydrogel
By designing polypeptides containing assembly-promoting and functionalized peptides and divalent manganese ions to self-assemble to form porous hydrogels, the problems of enzymatic degradation and insufficient therapeutic properties of the polypeptide system in cancer treatment are solved, and long-term drug molecules are realized. Effective retention and sustained release significantly enhance the effect of tumor immunotherapy.
Patent Information
- Application Number
- CN202410844405.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
Existing peptide systems have enzymatic degradation and limited therapeutic properties in cancer treatment, making it difficult to effectively regulate immune responses and improve anti-tumor effects.
By designing polypeptides containing peptides that promote assembly and functionalization, metal ions such as divalent manganese ions are used to self-assemble to form a hydrogel with a porous structure and a fibrous network structure, which is combined with drug molecules to form a delivery carrier to achieve long-term retention and relief. release.
It improves the stability and cancer cell killing effect of the anti-tumor tripeptide YSV, achieves long-term retention and sustained release of metal ions and drug molecules, and significantly enhances the efficacy of tumor immunotherapy.
Smart Images

Figure CN118772233A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of biomaterials, and in particular to a polypeptide for preparing hydrogel, polypeptide hydrogel and a preparation method and application thereof. Background Art
[0002] Cancer immunotherapy is a revolution in cancer treatment that uses the patient's own immune system to fight the occurrence and development of tumors. Strategies such as immune checkpoint blockade (ICB), T cell adoptive therapy, and cancer vaccines are becoming mainstream methods for cancer treatment. Since "cold" tumors usually have an immunosuppressive tumor microenvironment (TME), including insufficient numbers of activated dendritic cells (DCs), insufficient tumor infiltration of cytotoxic T lymphocytes (CTLs), and increased immunosuppressive cells, some immunotherapies face the problem of low patient response rates.
[0003] A variety of immunotherapeutic drugs, such as STING agonists, TLR agonists, cytokines, and immune checkpoint inhibitors have been tested in preclinical and clinical trials. Systemically administered immunotherapies can cause immune-related side effects during tumor treatment, and it is difficult to maintain effective drug concentrations at the tumor site, while locally administered soluble preparations cannot effectively accumulate at the tumor site due to rapid drug metabolism. Therefore, smart delivery systems are needed to change the biodistribution of immunotherapies, achieve spatiotemporally controlled cargo release, and induce an immune-stimulating tumor microenvironment, which is beneficial for improving the safety and efficacy of immunotherapy.
[0004] Hydrogels are very attractive "smart" drug delivery systems that can achieve site-specific delivery of various bioactive drugs while achieving controlled and sustainable drug release. Hydrogels for local immunotherapy are not just drug reservoirs, they can also actively recruit endogenous immune cells to cultivate immunogenic niches. Local administration routes can enhance drug targeting, minimize rapid degradation of therapeutic drugs, and prevent systemic side effects.
[0005] Peptide-based molecules have inherent biocompatibility, sequence designability, and microstructural controllability, and can self-assemble to form hydrogels under specific conditions, including pH, temperature, ions, and enzymes, without the need for additional chemical reagents. As research and exploration continue to deepen, peptide-based self-assembly plays a role in cancer treatment in a variety of ways, including killing tumors, capturing tumor antigens, and activating immune cells, and has broad application prospects in anti-cancer. However, easy enzymatic degradability and limited cancer therapeutic properties limit their application.
[0006] CN110229215A discloses a drug sustained-release polypeptide hydrogel and its preparation method and use. The polypeptide hydrogel is prepared by mixing a self-assembling peptide aqueous solution, a heparin sodium aqueous solution, a hepatocyte growth factor (HGF) aqueous solution and a TNF-ɑ antibody (anti-TNF-ɑ). The hydrogel has good drug sustained-release effect and renal biocompatibility. By adding heparin sodium, the purpose of sequentially releasing anti-TNF-ɑ and HGF is achieved, and the apoptosis of renal tubular cells after acute renal injury can be effectively inhibited.
[0007] CN116966135A discloses a pH-responsive polypeptide drug sustained-release hydrogel and a preparation method thereof, wherein the polypeptide drug sustained-release hydrogel is a hydrogel in which a double cross-linked network is formed by aldehyde-modified negatively charged polymer, polypeptide drug and polyamino polymer cross-linking agent through aldehyde-amino Schiff base reaction and amino-negatively charged group ion interaction. The prepared hydrogel can realize the slow release and controlled release of polypeptide drugs, and has sensitive pH responsiveness, thereby controlling the drug release amount and realizing long-term treatment.
[0008] In summary, how to rationally design the polypeptide system, improve the availability of polypeptides, regulate immune responses, and enhance anti-tumor effects has become one of the urgent problems to be solved in this field. Summary of the invention
[0009] To solve the above technical problems, the present invention provides a polypeptide for preparing a hydrogel, a polypeptide hydrogel, and a preparation method and application thereof. The polypeptide can form a polypeptide hydrogel through self-assembly, and the polypeptide hydrogel has long-lasting retention and sustained release properties, thereby improving the tumor immune microenvironment and enhancing the tumor immunotherapy effect.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a polypeptide for preparing a hydrogel, wherein the polypeptide comprises an assembly-promoting peptide segment and a functionalized peptide segment; the amino acid sequence of the assembly-promoting peptide segment comprises Phe-Phe.
[0012] The present invention provides a polypeptide which can self-assemble with the help of metal ions to form a fibrous network structure hydrogel with a porous structure, and the peptide segments that promote assembly help form the hydrogel structure.
[0013] Preferably, the functionalized peptide segment has any one or at least two functions of targeting, anti-tumor, immune activation or blocking.
[0014] Preferably, the amino acid sequence of the functionalized peptide segment includes Tyr-Ser-Val.
[0015] The functionalized peptide segment YSV provided in the present invention has an anti-tumor effect.
[0016] Preferably, the amino acid sequence of the polypeptide includes the sequence shown in SEQ ID NO.1.
[0017] SEQ ID NO.1: FFYSV.
[0018] Preferably, an aromatic group is connected to the N-terminus of the polypeptide.
[0019] Preferably, the aromatic group includes any one of naphthyl, phenyl, pyrenyl or fluorenylmethoxycarbonyl.
[0020] Preferably, the N-terminus of the polypeptide is linked to 2-naphthylacetic acid (Nap).
[0021] Preferably, the method for preparing the polypeptide for preparing the hydrogel is a polypeptide solid phase synthesis-Fmoc synthesis method, comprising the following steps:
[0022] (1) Swelling of 2-chlorotrityl chloride resin;
[0023] (2) coupling of the first amino acid;
[0024] (3) Quenching of resin active sites;
[0025] (4) Removal of Fmoc protection and extension of the peptide chain;
[0026] (5) Capping of the N-terminus of the polypeptide chain;
[0027] (6) cleavage of the polypeptide from the resin;
[0028] (7) The peptide was purified by HPLC.
[0029] In a second aspect, the present invention provides use of the polypeptide for preparing a hydrogel as described in the first aspect in preparing a hydrogel.
[0030] In a third aspect, the present invention provides a polypeptide hydrogel, wherein the polypeptide hydrogel comprises the polypeptide for preparing the hydrogel according to the first aspect.
[0031] Preferably, the polypeptide hydrogel further comprises metal ions.
[0032] Preferably, the metal ion includes any one of manganese ion, calcium ion, magnesium ion, copper ion, zinc ion, aluminum ion or iron ion, or a combination of at least two of them, preferably divalent manganese ion.
[0033] Preferably, the molar ratio of the polypeptide to the metal ion is 1:(5-30), preferably 1:(10-20).
[0034] The specific point values of 5-30 mentioned above can be selected from 5, 10, 15, 20, 25 or 30 etc.
[0035] The specific point values of 10-20 mentioned above can be selected as 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, etc.
[0036] In a fourth aspect, the present invention provides a method for preparing the polypeptide hydrogel as described in the third aspect, wherein the method for preparing the polypeptide hydrogel comprises the following steps:
[0037] (1) dissolving the polypeptide for preparing the hydrogel described in the first aspect in water to obtain a polypeptide aqueous solution, adjusting the pH with an alkaline solution, and vortexing and shaking until the polypeptide is completely dissolved;
[0038] (2) adding a metal salt aqueous solution dropwise under ultrasound, sonicating, and allowing to stand to obtain the polypeptide hydrogel.
[0039] Preferably, the concentration of the polypeptide in the polypeptide aqueous solution in step (1) is 1-10 mg / mL (e.g., 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL or 10 mg / mL, etc.).
[0040] Preferably, the alkaline solution in step (1) comprises any one of sodium hydroxide, ammonia water, sodium carbonate or sodium bicarbonate, or a combination of at least two thereof.
[0041] Preferably, the pH of the alkaline solution in step (1) is adjusted to 7.5-8.5 (e.g., 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4 or 8.5, etc.).
[0042] To ensure that the polypeptide is fully dissolved, the pH of the solution is adjusted to 7.5-8.5.
[0043] Preferably, the metal salt in step (2) comprises a divalent manganese salt.
[0044] In order to promote the self-assembly of polypeptide molecules to form a stable hydrogel, the present invention uses divalent manganese ions, a cGAS-STING pathway activator, to self-assemble under the action of the immune metal divalent manganese ions.
[0045] Preferably, the divalent manganese salt includes any one of manganese chloride, manganese nitrate, manganese sulfate or manganese acetate, or a combination of at least two thereof.
[0046] Preferably, the concentration of the aqueous metal salt solution is 0.1-5 mol / L (e.g., 0.1 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L or 5 mol / L, etc.), preferably 0.5-1 mol / L (e.g., 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L or 1 mol / L, etc.).
[0047] Preferably, the ultrasonic time in step (2) is 15-60 min (e.g., 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, etc.), preferably 20-30 min (e.g., 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min or 30 min, etc.).
[0048] Preferably, the temperature of the ultrasound in step (2) is 20-60°C (e.g., 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C, etc.), preferably 20-30°C (e.g., 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C or 30°C, etc.).
[0049] Preferably, the power of the ultrasound in step (2) is 150-250 W (e.g., 150 W, 160 W, 170 W, 180 W, 190 W, 200 W, 210 W, 220 W, 230 W, 240 W or 250 W, etc.).
[0050] In order to ensure that the divalent manganese ions and the polypeptide are fully cross-linked to form a stable homogeneous hydrogel, the present invention sets specific ultrasonic parameters.
[0051] In a fifth aspect, the present invention provides use of the polypeptide for preparing a hydrogel as described in the first aspect and / or the polypeptide hydrogel as described in the third aspect in preparing a drug molecule delivery carrier.
[0052] The polypeptide hydrogel provided by the present invention can be used for tumor immunotherapy. Since metal ions are slowly released from the gel, immune-related pathways can be activated, thereby achieving the effect of metal immunotherapy. In addition, the gel system can load drug molecules, prolong the retention time of drug molecules, achieve slow release of drug molecules, and synergistically enhance the efficacy of tumor immunotherapy with metal ions.
[0053] In a sixth aspect, the present invention provides a drug molecule delivery carrier, wherein the drug molecule delivery carrier comprises the polypeptide for preparing the hydrogel according to the first aspect and / or the polypeptide hydrogel according to the third aspect.
[0054] Preferably, the drug molecule delivery carrier further comprises drug molecules.
[0055] Preferably, the drug molecule comprises any one of a chemotherapeutic drug, a protein active molecule or an immunomodulatory molecule, or a combination of at least two of them.
[0056] Preferably, the drug molecule is an anti-PD-1 antibody.
[0057] Preferably, the drug molecule delivery carrier has the effect of drug retention and / or drug sustained release.
[0058] Preferably, the drug molecule delivery carrier has a tumor therapeutic effect.
[0059] Preferably, the tumor comprises a solid tumor.
[0060] Preferably, the solid tumor comprises any one of liver cancer, lung cancer, breast cancer, glioma, colon cancer or melanoma, or a combination of at least two thereof.
[0061] Preferably, the method for preparing the drug molecule delivery carrier comprises the following steps:
[0062] (1) dissolving the polypeptide for preparing the hydrogel described in the first aspect in water to obtain a polypeptide aqueous solution, adjusting the pH with an alkaline solution, and vortexing and shaking until the polypeptide is completely dissolved;
[0063] (2) Add drug molecules to the polypeptide aqueous solution and vortex until fully dissolved;
[0064] (3) adding a metal salt aqueous solution dropwise under ultrasound, sonicating, and allowing to stand to obtain the drug molecule delivery carrier.
[0065] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0066] Compared with the prior art, the present invention has the following beneficial effects:
[0067] (1) The polypeptide provided by the present invention can self-assemble with the help of metal ions to form a fibrous network structure hydrogel with a porous structure, which can be used to load drugs. The metal ions are preferably divalent manganese ions;
[0068] (2) The polypeptide hydrogel provided by the present invention can improve the stability and cancer cell killing effect of the anti-tumor tripeptide YSV, and can achieve long-term retention of metal ions and loaded bioactive molecules in the body and sustained release of drugs through local administration;
[0069] (3) The polypeptide hydrogel provided by the present invention is used in combination with anti-PD-1 antibodies to effectively inhibit tumor growth and show good anti-tumor immune effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 The photos show that different divalent manganese ion compounds promote the sol-gel transition of peptides;
[0071] Figure 2 This is a gel picture of peptide molecules and manganese ions at different molar ratios;
[0072] Figure 3 is a scanning electron micrograph of the polypeptide hydrogel;
[0073] Figure 4 This is the rheological data result diagram of polypeptide hydrogel;
[0074] Figure 5 This is a graph showing the results of HPLC analysis of the stability of polypeptide hydrogel against enzyme degradation;
[0075] Figure 6 This is a graph showing the results of measuring the critical aggregation concentration of polypeptide molecules and polypeptide hydrogels using the fluorescent probe thioflavin T;
[0076] Figure 7 Fourier transform infrared spectra of peptides and peptide hydrogels;
[0077] Figure 8 The circular dichroism spectra of the peptide and peptide hydrogel and the content analysis results of different secondary structures of the peptide before and after assembly are shown;
[0078] Fig. 9 Gel formation diagram of adding different metal ions to peptides;
[0079] Fig.10 This is the result of CCK-8 test on liver cancer cells after material treatment;
[0080] Fig.11 This is the result of Annexin V / PI detection of apoptosis of liver cancer cells after material treatment;
[0081] Fig.12 Representative flow cytometry images and quantitative analysis results of the proportion of mature BMDCs after material treatment;
[0082] Fig.13 Representative flow cytometry images and quantitative analysis results of BMDM polarization into M1 macrophages after material treatment;
[0083] Fig.14The figures are the analysis results at different time points after intratumoral injection of free MnCl2 solution and polypeptide hydrogel, wherein figure a is the retention of manganese ions in the tumor at different time points after intratumoral injection of free MnCl2 solution and polypeptide hydrogel, and figure b is the ICP-MS analysis results of manganese ions in various organs of mice at different time points after intratumoral injection of MnCl2 or polypeptide hydrogel;
[0084] Fig.15 The images and fluorescence intensity quantitative results of the tumor sites at different time points after intratumoral injection of free Cy5.5-anti-PD-1 antibody solution and peptide hydrogel loaded with Cy5.5-anti-PD-1 antibody;
[0085] Fig.16 The following are the results of the survival analysis of mice in different groups after treatment, wherein Figure a is the tumor growth curve of mice in different groups after treatment, Figure b is the tumor image and weight result image of mice in different groups on the 15th day after treatment, and Figure c is the survival rate result image of mice in different groups after treatment;
[0086] Fig.17 This is the result of flow cytometry analysis of the ratio of mature DCs, M1 / M2 macrophages, NK cells and T cells in the tumors of mice in different groups after treatment;
[0087] Fig.18 The figure is the curve of the weight change of mice after different drug treatments;
[0088] Fig.19 The histological HE staining images of the main organs of mice after different drug treatments;
[0089] Fig. 20 This is a statistical graph of blood biochemical indices of mice after different drug treatments. DETAILED DESCRIPTION
[0090] To further illustrate the technical means and effects of the present invention, the present invention is further described below in conjunction with the embodiments and drawings. It should be understood that the specific implementation methods described herein are only used to explain the present invention, rather than to limit the present invention.
[0091] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0092] Example 1
[0093] In this example, a polypeptide molecule Nap-FFYSV was prepared, and the preparation method included the following steps:
[0094] (1) Swelling of 2-chlorotrityl chloride resin;
[0095] A certain amount of 2-chlorotrityl chloride resin (1.190 mmol / g) was weighed and placed in a peptide solid phase synthesis tube, swollen with dry dichloromethane (DCM) for 20 min under nitrogen, then washed three times with dry N,N-dimethylformamide (DMF), and then dried for standby use.
[0096] (2) coupling of the first amino acid;
[0097] Take 2 times the equivalent of L-Fmoc-Val-OH and 4 times the equivalent of N,N-diisopropylethylamine (DIPEA) relative to the resin, dissolve them in DMF, add them into the solid phase synthesis tube, react for 1 hour under nitrogen bubbling, and wash with DMF. Use ultraviolet to monitor whether there are any residual amino acids, so that the first amino acid can be connected to the resin.
[0098] (3) Quenching of resin active sites;
[0099] Prepare resin blocking solution: dichloromethane (DCM), methanol (MeOH), N,N-diisopropylethylamine (DIPEA) in a ratio of 16:3:1. Quench the resin with blocking solution twice for a total of 20 min, and then wash it with DMF.
[0100] (4) Removal of Fmoc protection and extension of the peptide chain;
[0101] Add a certain amount of 20% piperidine solution to the reactor, react for 20 minutes, filter out the reaction solution after completion, wash with DMF, and monitor whether there are any residual Fmoc groups using UV. Take 2 times the equivalent of L-Fmoc-Ser(tBu)-OH, 4 times the equivalent of DIPEA, and 3 times the equivalent of HBTU relative to the resin, dissolve them in DMF, add them to the solid phase synthesis tube, react for 1 hour under nitrogen bubbling, and wash with DMF, and monitor whether there are any residual amino acids using UV, so that the second amino acid is connected to the resin. According to the peptide chain amino acid sequence, repeat the above steps of deprotection and coupling until the last amino acid is synthesized to obtain a resin connected to a polypeptide chain.
[0102] (5) Capping of the N-terminus of the polypeptide chain;
[0103] Take 2 times the equivalent of 2-naphthylacetic acid and 4 times the equivalent of DIPEA relative to the resin, dissolve them in DMF, add them into the reactor and react for 2 hours to cap the N-terminus. After the reaction, wash with DMF.
[0104] (6) cleavage of the polypeptide from the resin;
[0105] The polypeptide was cleaved from the resin using a cleavage solution, trifluoroacetic acid (TFA), and the side chain protection of the amino acid was removed. TFA was removed by rotary evaporation and crudely precipitated with ice ether to obtain a crude product of the target polypeptide.
[0106] (7) Purification of polypeptides.
[0107] The crude polypeptide is separated and purified by reverse phase preparative liquid chromatography (HPLC), and then freeze-dried to obtain a polypeptide with a purity higher than 95%.
[0108] Example 2
[0109] In this embodiment, a polypeptide hydrogel is prepared, and the preparation method comprises the following steps:
[0110] (1) The purified Nap-FFYSV polypeptide molecules were dissolved in water, and the pH value of the polypeptide solution was adjusted to 7.5 with 1 M NaOH. The solution was further vortexed until dissolved to form a polypeptide solution with a concentration of 4 mg / mL.
[0111] (2) Then, slowly add 1 M manganese chloride, manganese acetate, manganese sulfate or manganese nitrate aqueous solution under ultrasound to make the molar ratio of polypeptide molecules to manganese ions 1:10, continue ultrasound for 30 minutes, and observe the formation of gel.
[0112] Figure 1 These are photos of the sol-gel transition of polypeptides after adding different divalent manganese salt solutions. The results show that the type of acid ions in the manganese salt solution does not affect the gelation effect of the hydrogel.
[0113] (3) To the 4 mg / mL polypeptide solution formed after dissolution in step (1), add an aqueous solution of manganese chloride in a molar amount of 5, 10, 15, 20, and 30 times that of the polypeptide, respectively, and continue ultrasonication for 30 min. The resulting solution is then left to stand and the formation of gel is observed.
[0114] Figure 2 The gel formation pictures of peptide and manganese ion at different molar ratios are shown. 2+ The hydrogel can be assembled when the molar ratio of the peptide to the peptide is in the range of 5-30.
[0115] In the following characterizations and examples, manganese chloride was used as a source of manganese ions, and the molar ratio of polypeptide to manganese ions was 1:10 for gelation and assembly.
[0116] Figure 3 The scanning electron microscope morphology of the porous network fiber structure of the gel; Figure 4 The rheological data of the hydrogel. The left figure shows the strain-dependent oscillatory shear rheology results of the hydrogel at a fixed frequency of 10 rad / s, and the right figure shows the dynamic frequency scanning results of the hydrogel measured at 0.1% strain.
[0117] Example 3
[0118] In this example, the polypeptide prepared in Example 1 and the polypeptide hydrogel prepared in Example 2 were diluted in water to a concentration of 0.3 mM, and proteinase K was added to a final concentration of 0.2 mg / mL. After a specific digestion time, an equal volume of methanol was added to stop the degradation of proteinase K. The samples were analyzed by HPLC to obtain a degradation graph over time.
[0119] Figure 5 The HPLC graphs of tripeptide YSV, polypeptide Nap-FFYSV (Pep) and polypeptide hydrogel (Pep-Mn gel) under the action of protease over time show that the YSV tripeptide is rapidly degraded within 2 hours, while the modified polypeptide and polypeptide hydrogel can maintain their initial structure for up to 24 hours, indicating that the improved material has improved resistance to rapid enzyme degradation.
[0120] Example 4
[0121] This example explores the mechanism by which metal ions promote the assembly of polypeptide hydrogels:
[0122] (1) Critical assembly concentration (CAC) test of hydrogel
[0123] Thioflavin T (ThT) was used as a probe molecule and the critical assembly concentration (CAC) of the peptide was determined by the fluorescent probe method. The peptide prepared in Example 1 was diluted with ultrapure water to form two concentration gradients of 1-700 μM. One portion was left to assemble at room temperature for 1 h, and the other portion was added with MnCl2 aqueous solution. The peptide and Mn 2+ The assembled material was mixed with 20 μM ThT at a molar ratio of 1:10 for 1 h, and the fluorescence intensity was measured at an excitation wavelength of 450 nm and an emission wavelength of 485 nm.
[0124] Figure 6 is the critical assembly concentration of the single polypeptide molecule and the polypeptide molecule after adding manganese ions. The results show that Mn 2+ The addition of effectively lowered the critical assembly concentration of the polypeptide and accelerated the formation of the assembly.
[0125] (2) Determination of the role of the peptide molecular skeleton in assembly based on Fourier transform infrared (FT-IR)
[0126] The polypeptide solution and the polypeptide hydrogel containing manganese ions in Example 2 were freeze-dried to obtain freeze-dried powders. The same mass of the powders were ground and mixed with potassium bromide (1:50) and pressed into disc-shaped samples. -1 The infrared spectrum was recorded within the scan range.
[0127] Figure 7 The Fourier transform infrared spectra (FT-IR) of the peptide and the peptide hydrogel containing manganese ions show that 3281cm -1 The NH absorption peak at 3290 cm -1 , and the peak becomes wider, 1500-1400cm- 1 The peak in the region is significantly broadened, indicating that Mn 2+ It promotes the formation of intermolecular hydrogen bonds between the amide groups of polypeptide molecules and enhances the π-π interaction of the side chain benzene ring.
[0128] (3) Determination of changes in the secondary structure of the molecule after Mn ion-induced peptide assembly based on circular dichroism (CD)
[0129] Prepare two 0.2 mg / mL peptide solutions according to Example 2, one of which contains 10 times the molar amount of Mn 2+ Both solutions were assembled at room temperature for 1 h after sonication and then transferred to a quartz cuvette and scanned at a scanning speed of 500 nm / min, a resolution of 0.5 nm, and a temperature of 25°C, and the secondary structure of the peptide was analyzed in the software.
[0130] Figure 8 The circular dichroism (CD) spectrum and secondary structure content analysis of the peptide assembled with manganese ions showed that when Mn was added to the peptide system 2+ When the concentration of β-folded secondary structure of the peptide increases, the change of secondary structure further induces the gelation of the peptide.
[0131] (4) Assembly of various metal ions and polypeptide molecules:
[0132] Gels assembled with polypeptides and different metal ions were prepared with reference to Example 2. The metal ions included monovalent, divalent and trivalent ions. The specific ion types and aqueous solution concentrations were: Na + (5mol / L), K + (1mol / L), Ca 2+ (5mol / L), Mg 2+ (1mol / L), Cu 2+ (2mol / L), Zn 2+ (0.8mol / L), Al 3+ (0.5mol / L), Fe 3+ (0.1mol / L). The molar ratio of polypeptide to metal ion is Na + (1:30), K + (1:28), Ca 2+ (1:18),Mg 2+(1:20), Cu 2+ (1:15), Zn 2+ (1:20), Al 3+ (1:5), Fe 3+ (1:10); After each metal ion is mixed with the polypeptide solution, the pH is adjusted using different alkaline solutions: Na + (adjust the pH value to 7.5 with ammonia water), K + (sodium carbonate adjusted to pH 8.5), Ca 2+ (adjust pH to 7.6 with ammonia), Mg 2+ (sodium bicarbonate adjusted to pH 7.9), Cu 2+ (sodium carbonate adjusted to pH 8.5), Zn 2+ (adjust the pH value of ammonia to 7.5), Al 3+ (adjusted to pH 7.5 with sodium carbonate), Fe 3+ (sodium bicarbonate was adjusted to pH 7.5); the specific conditions for ultrasonic treatment were as follows: Na + (150W, 20℃, 60min treatment), K + (250W, 60℃, 15min treatment), Ca 2+ (200W, 40℃, 20min treatment), Mg 2+ (180W, 40℃, 30min treatment), Cu 2+ (250W, 60℃, 15min treatment), Zn 2+ (150W, 20℃, 60min treatment), Al 3+ (200W, 50℃, 20min treatment), Fe 3+ (220W, 30℃, treatment for 30min).
[0133] Fig. 9 This is the gel assembly situation of polypeptides and different metal ions, among which divalent and trivalent ions promote the formation of gel more significantly than monovalent ions. The specific reason is that the higher valence state of metal ions leads to a stronger coordination effect with polypeptide molecules.
[0134] Example 5
[0135] This example tests the in vitro tumor cell killing effect of polypeptide hydrogels:
[0136] (1) CCK-8 cytotoxicity assay:
[0137] HepG2 cells were cultured at 1×10 4Cells / well were inoculated into a 96-well plate, and after overnight attachment, different doses of the polypeptide hydrogel prepared in Example 2 were added and incubated for 24 hours. The culture medium containing the material was then removed, and a culture medium containing 10% CCK-8 reagent was added, and the cells were incubated at 37°C until the cells in the well turned yellow. The cell viability was evaluated by detecting the excitation of visible light at 450nm and the absorption value at 600nm, and three replicate wells were set for each group.
[0138] Fig.10 The results of the cell viability test showed that the gel showed a stronger cancer cell killing effect compared with the control group YSV peptide and Nap-FFYSV peptide.
[0139] (2) Annexin V / PI double staining method to detect cell apoptosis:
[0140] HepG2 cells were taken at 5×10 5 Cells / well were inoculated in a 6-well plate, and after overnight attachment, the polypeptide hydrogel prepared in Example 2 (polypeptide concentration: 40 μM, manganese ion concentration: 400 μM) was added and incubated for 24 hours. The cells were then collected, stained with fluorescent dyes Annexin V and PI, and then the apoptosis of cancer cells was detected by flow cytometry. Three replicate wells were set for each group.
[0141] Fig.11 The effects of different materials on apoptosis of HepG2 cells showed that the gel exhibited the most obvious apoptosis level of cancer cells compared with YSV peptide and Nap-FFYSV peptide.
[0142] Example 6
[0143] This example is used to test the stimulating effect of polypeptide hydrogel on immune cells in vitro:
[0144] (1) Bone marrow-derived dendritic cell (BMDC) activation experiment:
[0145] BMDCs were extracted from the femur and tibia of mice. On the 8th day of cell culture, BMDCs were cultured at a concentration of 1×10 6 Cells / well were inoculated into a 6-well plate and then incubated for 24 hours with the polypeptide hydrogel (polypeptide concentration: 30 μM, manganese ion concentration: 300 μM) prepared in Example 2. BMDC cells were then harvested and the maturity of DC cells was detected by flow cytometry.
[0146] The culture conditions of the BMDCs are: RPMI 1640 medium containing 10% FBS, 1% penicillin-streptomycin, 20 ng / mL GM-CSF and 10 ng / mL IL-4, and half of the medium is replaced every 2 days.
[0147] Fig.12Representative flow cytometry images and quantitative analysis of the proportion of mature BMDCs after treatment with different materials. The results showed that compared with the administration of tripeptide, polypeptide and manganese ions alone, polypeptide hydrogel significantly upregulated the proportion of CD80 and CD86 on BMDCs.
[0148] (2) Bone marrow-derived macrophage (BMDM) polarization experiment:
[0149] BMDM cells were extracted from the femur and tibia of mice. On the sixth day of cell culture, BMDM cells were cultured at a concentration of 1×10 6 Cells / well were inoculated into a 6-well plate and then incubated for 24 hours with the polypeptide hydrogel prepared in Example 2 (polypeptide concentration: 30 μM, manganese ion concentration: 300 μM). BMDM cells were then harvested and the proportion of M1 macrophages was detected by flow cytometry.
[0150] The culture conditions of the BMDM are: DMEM culture medium containing 10% FBS, 1% penicillin-streptomycin and 20ng / mL M-CSF, and half of the culture medium is replaced every 3 days.
[0151] Fig.13 Representative flow cytometry images and quantitative analysis of BMDM polarization into M1 macrophages after treatment with different materials. The results showed that peptide hydrogel and Mn 2+ The group showed a significantly higher ability to polarize to the M1 phenotype than the other groups.
[0152] Example 7
[0153] This example demonstrates that polypeptide hydrogel achieves retention and sustained release of manganese ions in vivo:
[0154] Balb / c female mice were injected subcutaneously with 2×10 6 H22 liver cancer cells were used to establish a mouse tumor-bearing model. When the average tumor volume of the mice grew to 200 mm 3 The mice were divided into two groups, one group was intratumorally administered with 50 μL of manganese chloride solution, and the other group was intratumorally administered with 50 μL of the polypeptide hydrogel prepared in Example 2, and the dose of manganese ions remained the same (100 μg / mouse). The mice were killed at specific time points (12h, 24h, and 48h), the tumors and organs were removed, and the manganese ion content in the tissues was tested by ICP-MS.
[0155] The ICP-MS sample processing steps of the tissue are as follows: the tissue is pre-digested in concentrated HNO3 at room temperature overnight, and the next day they are heated to 180°C on a graphite hot plate, and H2O2 is gradually added until the tissue sample is completely digested. Next, the solution is heated to 230°C to remove residual HNO3. Finally, the remaining colorless solution is diluted to 3 mL with 2% HNO3 for ICP-MS analysis.
[0156] Fig.14 Figure a in the middle shows the retention of manganese ions in the tumor at different time points after intratumoral injection of free MnCl2 solution and polypeptide hydrogel. Fig.14 Figure b shows the content of manganese ions in various organs of mice at different time points after intratumoral injection of MnCl2 or polypeptide hydrogel. The results show that the hydrogel retains more manganese ions at the tumor site at different time points, achieving sustained release of manganese ions. The manganese ions injected into the tumor are mainly metabolized by the kidneys, and the content gradually decreases over time.
[0157] Example 8
[0158] This example demonstrates that polypeptide hydrogels can be used as carriers for chemotherapeutic drugs, such as doxorubicin, paclitaxel, cisplatin, etc., as well as protein active molecules or immunomodulatory molecules, such as anti-PD-1 antibodies, RBD sequences, cytokines IL-12, IL-2, etc.
[0159] Take anti-PD-1 antibody as an example to prepare the carrier hydrogel:
[0160] (1) The purified Nap-FFYSV polypeptide molecules were dissolved in water, and the pH value of the polypeptide solution was adjusted to 7.5 with 1 M NaOH. The solution was further vortexed until dissolved to form a polypeptide solution with a concentration of 4 mg / mL.
[0161] (2) Add anti-PD-1 antibody to the peptide solution and continue vortexing until it is fully dissolved and mixed evenly.
[0162] (3) Then, 1 M manganese chloride was slowly added dropwise under ultrasound to make the molar ratio of polypeptide molecules to manganese ions 1:10, and ultrasound was continued for 30 min. After that, the mixture was allowed to stand for more than 6 hours. The formation of gel could be observed.
[0163] Furthermore, the anti-PD-1 antibody hydrogel carrier achieves sustained release of anti-PD-1 antibodies in vivo:
[0164] Balb / c female mice were injected subcutaneously with 2×10 6 H22 liver cancer cells were used to establish a mouse tumor-bearing model. When the average tumor volume of the mice grew to 200 mm 3 At the same time, the mice were divided into two groups. One group was intratumorally administered with 50 μL Cy5.5-labeled anti-PD-1 antibody solution (αPD-1-Cy5.5), and the other group was intratumorally administered with 50 μL Cy5.5-labeled anti-PD-1 antibody peptide hydrogel (αPD-1-Cy5.5@Pep-Mn gel). The dose of anti-PD-1 antibody remained the same (25 μg / mouse). At specific time points (12h, 24h, 48h, 72h, 96h, 168h), the mice were killed, the tumors were removed, and the antibody fluorescence intensity at the tumor site was analyzed by IVIS.
[0165] Fig.15 Fluorescence imaging pictures and fluorescence intensity quantification of tumor sites at different time points after intratumoral injection of free Cy5.5-anti-PD-1 antibody solution and peptide hydrogel loaded with Cy5.5-anti-PD-1 antibody. The results showed that peptide hydrogel extended the tumor retention time of anti-PD-1 antibody to 168h, while the antibody in the free solution group had almost no detectable fluorescence signal at 96h, indicating that the free group antibody leaked from the tumor tissue faster.
[0166] Example 9
[0167] This example tests the in vivo anti-tumor effect of polypeptide hydrogel loaded with anti-PD-1 antibody:
[0168] Balb / c female mice were injected subcutaneously with 2×10 6 H22 liver cancer cells were used to establish a mouse tumor-bearing model. When the average tumor volume of the mice grew to 100 mm 3 The patients were divided into six groups (G1: untreated group, G2: Nap-FFYSV group, G3: MnCl2 solution group, G4: anti-PD-1 antibody solution group, G5: polypeptide hydrogel group, G6: polypeptide hydrogel loaded with anti-PD-1 antibody group). The intratumoral administration (polypeptide: 150 μg; MnCl2 solution ... 2+ : 100μg; αPD-1: 50μg), and the administration was carried out three times. The tumor volume of the mice was monitored every other day during the administration period. Two days after the last administration, the mice were killed, and the tumors were removed, photographed, and weighed.
[0169] Fig.16 Figure a in the middle shows the tumor growth curves of mice in different groups after treatment. Fig.16 Figure b in the middle shows the tumor photo and weight on the 15th day. Fig.16 Figure c in the middle shows the survival rate of mice after treatment in different groups. The results showed that the gel group (G5 and G6) showed the best tumor growth inhibition effect, and the tumor growth rate in the G6 group was slower than that in the G5 treatment group, indicating that the synergistic effect of anti-PD-1 antibody and gel produced a more excellent therapeutic effect. The free solution (G2, G3 and G4) treatment showed limited inhibitory effect on tumor growth. In addition, when the gel was combined with the anti-PD-1 antibody, the survival benefit of mice was the greatest.
[0170] Example 10
[0171] This example explores the regulation of the tumor immune microenvironment by polypeptide hydrogels:
[0172] Two days after the last administration in Example 9, mice were killed and tumor tissues were removed. The tumor tissues were cut into small pieces, and type IV collagenase (1 mg / mL) was added and shaken on a shaker at 37°C for 1 h, and then single cells were harvested through a 70 μm filter. The proportions of mature DCs, macrophages, NK cells, and T cells in the tumor were detected by flow cytometry.
[0173] Fig.17 The ratio of mature DC, M1 / M2 macrophages, NK cells and T cells in the tumor of mice after treatment in different groups. The results showed that the hydrogel group (G5 and G6) increased the proportion of immune cells compared with other groups and induced more immune cells to infiltrate the tumor.
[0174] Embodiment 11
[0175] This example is used to demonstrate the biosafety of polypeptide hydrogel preparations in mice:
[0176] (1) Mouse weight monitoring:
[0177] The body weights of the mice in different groups in Example 9 were monitored every other day.
[0178] Fig.18 Figure 2 is the body weight change curve of mice after different drug treatments. The results showed that no significant weight loss occurred in all groups during the treatment.
[0179] (2) Safety evaluation of major organs in mice:
[0180] Two days after the completion of the intratumoral drug administration treatment in Example 9, the mice were killed, and the main organs (heart, liver, spleen, lung, and kidney) were fixed in 4% paraformaldehyde for 48 h, and then the tissues were dehydrated, embedded, and sliced for hematoxylin-eosin (HE) staining.
[0181] Fig.19 This is the histological HE staining of the main organs of mice after different drug treatments. The results show that no obvious inflammatory infiltration or side effects were found in the tissues after gel treatment.
[0182] (3) Blood biochemical indicators of mice:
[0183] Two days after the intratumoral administration treatment in Example 9, the mice were killed, and blood and serum were taken for blood routine and blood biochemical index tests. The specific indexes were: alanine aminotransferase (ALT), aspartate aminotransferase (AST), blood urea nitrogen (BUN), creatinine (CREA), red blood cell count (RBC), white blood cell count (WBC), platelet count (PLT), and hemoglobin concentration (HGB).
[0184] Fig. 20These are the blood biochemical indices of mice after different drug treatments. The results showed that the serum biochemical parameters of mice remained at normal levels after gel treatment, and no abnormalities were found in the results of complete blood cell analysis.
[0185] In summary, the present invention provides a polypeptide hydrogel containing divalent manganese ions and a preparation method thereof, wherein a polypeptide of a specific sequence and divalent manganese ions cooperate to form a polypeptide hydrogel through self-assembly, and the assembled hydrogel has a fibrous porous structure, which can be further used as a carrier for drug delivery, and has long-term retention and sustained release properties. The present invention also relates to the use of the combination of the gel system and a drug in cancer immunotherapy, especially liver cancer treatment.
[0186] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A polypeptide for preparing a hydrogel, characterized in that: The polypeptide contains a peptide segment that promotes assembly and a functionalized peptide segment; the amino acid sequence of the peptide segment that promotes assembly includes Phe-Phe.
2. The polypeptide according to claim 1, characterized in that The functionalized peptide segment has any one or at least two functions of targeting, anti-tumor, immune activation or blocking; Preferably, the amino acid sequence of the functionalized peptide segment includes Tyr-Ser-Val; Preferably, the amino acid sequence of the polypeptide includes the sequence shown in SEQ ID NO.1; Preferably, the N-terminus of the polypeptide is connected to an aromatic group; Preferably, the aromatic group includes any one of naphthyl, phenyl, pyrenyl or fluorenylmethoxycarbonyl; Preferably, the N-terminus of the polypeptide is linked to 2-naphthylacetic acid.
3. Use of the polypeptide for preparing hydrogel according to claim 1 or 2 in preparing hydrogel.
4. A polypeptide hydrogel, characterized in that: The polypeptide hydrogel comprises the polypeptide for preparing the hydrogel according to claim 1 or 2.
5. The polypeptide hydrogel according to claim 4, characterized in that The polypeptide hydrogel further comprises metal ions; Preferably, the metal ion includes any one of manganese ion, calcium ion, magnesium ion, copper ion, zinc ion, aluminum ion or iron ion or a combination of at least two thereof, preferably divalent manganese ion; Preferably, the molar ratio of the polypeptide to the metal ion is 1:(5-30), preferably 1:(10-20).
6. A method for preparing the polypeptide hydrogel according to claim 4 or 5, characterized in that: The preparation method of the polypeptide hydrogel comprises the following steps: (1) dissolving the polypeptide for preparing a hydrogel according to claim 1 or 2 in water to obtain an aqueous polypeptide solution, adjusting the pH with an alkaline solution, and vortexing the solution until the polypeptide is completely dissolved; (2) adding a metal salt aqueous solution dropwise under ultrasound, sonicating, and allowing to stand to obtain the polypeptide hydrogel.
7. The method for preparing the polypeptide hydrogel according to claim 6, characterized in that: The concentration of the polypeptide in the polypeptide aqueous solution in step (1) is 1-10 mg / mL; Preferably, the alkaline solution in step (1) comprises any one of sodium hydroxide, ammonia water, sodium carbonate or sodium bicarbonate, or a combination of at least two thereof; Preferably, the pH of the alkaline solution in step (1) is adjusted to 7.5-8.5; Preferably, the metal salt in step (2) comprises a divalent manganese salt; Preferably, the divalent manganese salt includes any one or a combination of at least two of manganese chloride, manganese nitrate, manganese sulfate or manganese acetate; Preferably, the concentration of the aqueous metal salt solution is 0.1-5 mol / L, preferably 0.5-1 mol / L; Preferably, the ultrasonication time in step (2) is 15-60 min, preferably 20-30 min; Preferably, the temperature of the ultrasound in step (2) is 20-60°C, preferably 20-30°C; Preferably, the power of the ultrasound in step (2) is 150-250W.
8. Use of the polypeptide for preparing a hydrogel according to claim 1 or 2 and / or the polypeptide hydrogel according to claim 4 or 5 in preparing a drug molecule delivery carrier.
9. A drug molecule delivery carrier, characterized in that: The drug molecule delivery carrier comprises the polypeptide for preparing the hydrogel according to claim 1 or 2 and / or the polypeptide hydrogel according to claim 4 or 5.
10. The drug molecule delivery carrier according to claim 9, characterized in that: The drug molecule delivery carrier also includes drug molecules; Preferably, the drug molecule comprises any one or a combination of at least two of a chemotherapeutic drug, a protein active molecule or an immunomodulatory molecule; Preferably, the drug molecule delivery carrier has the effect of drug retention and / or drug sustained release; Preferably, the drug molecule delivery carrier has a tumor treatment effect; Preferably, the tumor comprises a solid tumor; Preferably, the solid tumor comprises any one or a combination of at least two of liver cancer, lung cancer, breast cancer, glioma, colon cancer or melanoma; Preferably, the method for preparing the drug molecule delivery carrier comprises the following steps: (1) dissolving the polypeptide for preparing a hydrogel according to claim 1 or 2 in water to obtain an aqueous polypeptide solution, adjusting the pH with an alkaline solution, and vortexing the solution until the polypeptide is completely dissolved; (2) Add drug molecules to the polypeptide aqueous solution and vortex until fully dissolved; (3) adding a metal salt aqueous solution dropwise under ultrasound, sonicating, and allowing to stand to obtain the drug molecule delivery carrier.
Citation Information
Patent Citations
Medicine slow release polypeptide hydrogel and preparation method and application thereof
CN110229215A
PH-responsive polypeptide drug sustained-release hydrogel and preparation method thereof
CN116966135A
Cited By
Iodine complex polypeptide antibacterial hydrogel as well as preparation method and application thereof
CN119431496A