A bio-based degradable nylon and preparation method thereof
By using degradable diamines and bio-based dibasic acids for polymerization, the existing bio-based degradable nylon preparation steps and poor performance were solved, and nylon materials with excellent degradation, mechanical and heat resistance were prepared. Suitable for large-scale production.
Patent Information
- Application Number
- CN202411260236.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The existing preparation methods for bio-based degradable nylon are complicated, and the obtained materials have poor mechanical properties and heat resistance, and high water absorption.
The polymerization reaction is carried out using degradable diamines and bio-based dibasic acids. Through specific temperature, pressure and catalyst control, bio-based degradable nylon with excellent degradation properties, good mechanical properties and heat resistance is prepared.
It has achieved efficient preparation of bio-based degradable nylon, with good degradation performance, excellent mechanical properties, low water absorption, and high yield and molecular weight, suitable for large-scale production.
Smart Images

Figure CN118772399B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials and relates to a bio-based degradable nylon and a preparation method thereof. Background Art
[0002] Nylon (PA) is a general term for polymers with amide groups (-CO-NH-), which can be formed by self-polymerization of lactam molecules or by polycondensation of diamines and dibasic acids. Its molecular structure is mainly composed of amide groups and methine or other cycloalkyl and aromatic groups. Nylon has good mechanical properties, heat resistance, wear resistance and self-lubricating properties, and is widely used in electronic appliances, automobiles, aerospace and other fields.
[0003] However, the polymerization monomers of nylon are generally derived from fossil fuels, which consume a large amount of oil resources. At present, the growth rate of proven oil reserves has slowed down significantly, the remaining production capacity is limited, and the extraction, refining, storage, transportation and use of oil are prone to damage the ecological environment. As the concept of sustainable development has become popular, the conversion and utilization of biomass raw materials has become a new research hotspot. Therefore, bio-based degradable nylon has received more and more attention from academia and industry in recent years.
[0004] However, the existing preparation methods of bio-based degradable nylon have the problems of complicated preparation steps, and the prepared degradable nylon has poor mechanical properties and poor heat resistance. Summary of the invention
[0005] In order to solve the defects in the prior art, the present invention provides a bio-based degradable nylon and a preparation method thereof. The obtained bio-based degradable nylon has excellent degradation performance, good mechanical properties and heat resistance, as well as low water absorption, high yield and molecular weight.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a bio-based degradable nylon, the raw materials for preparing the nylon include a degradable diamine and a bio-based dibasic acid;
[0008] The degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine, and 3,3'-dithiobispropylamine;
[0009] The bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid.
[0010] Preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:(0.6-1.2). More preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:1.
[0011] Preferably, the degradable diamine is 4,4'-dithiodiphenylamine.
[0012] Preferably, the bio-based dibasic acid is 2,5-furandicarboxylic acid.
[0013] Preferably, the structural formula of the bio-based degradable nylon is as shown in Formula I below:
[0014]
[0015] Formula I.
[0016] Preferably, the number average molecular weight of the bio-based degradable nylon is 55,000-61,000.
[0017] In a second aspect, the present invention provides a method for preparing bio-based degradable nylon, comprising the following steps:
[0018] S1. Mixing a degradable diamine, a bio-based dibasic acid and a solvent in a protective atmosphere to obtain a mixture; the degradable diamine is selected from at least one of 4,4'-dithiodiphenylamine, 2,2'-dimethoxy-4,4'-dithiodiphenylamine and 3,3'-dithiobispropylamine; the bio-based dibasic acid is selected from at least one of 2,5-furandicarboxylic acid, 2-hydroxysuccinic acid, itaconic acid, malonic acid, succinic acid, glutaric acid, adipic acid and sebacic acid;
[0019] S2, stirring the mixture under elevated temperature, stopping the temperature increase after reaching the target temperature and pressurizing to carry out condensation reaction to obtain reactant 1;
[0020] S3, subjecting the reactant 1 to a reaction after gradually increasing the temperature under a pressurized environment to obtain a reactant 2;
[0021] S4, releasing the pressure of the reactant 2, raising the temperature, and reacting in a vacuum environment to obtain bio-based degradable nylon.
[0022] Preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:(0.6-1.2); more preferably, the molar ratio of the degradable diamine to the bio-based dibasic acid is 1:1.
[0023] Preferably, the mass of the solvent accounts for 50-70% of the sum of the mass of the degradable diamine and the bio-based dibasic acid.
[0024] Preferably, the protective atmosphere in S1 is selected from any one of nitrogen, argon, helium and neon.
[0025] Preferably, a catalyst is also added to S1.
[0026] Preferably, the catalyst is selected from at least one of sodium hypophosphite, sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, phosphate ester, propyl titanate, and boric acid.
[0027] Preferably, the mass of the catalyst accounts for 0.15-0.31% of the sum of the mass of the degradable diamine and the bio-based dibasic acid.
[0028] Preferably, the stirring speed in S2 is 300-400 r / min, and the target temperature is 140-170 °C.
[0029] Preferably, the pressurized pressure in S2 is 0.5-0.9 Mpa.
[0030] Preferably, the reaction time of the S2 condensation reaction is 2 to 4 h.
[0031] Preferably, the gradient heating condition in S3 is: heating to 270-310° C. at a heating rate of 20-40° C. / min.
[0032] Preferably, the pressure of the pressurized environment in S3 is 3-4 Mpa.
[0033] Preferably, the reaction time in S3 is 1 to 3 h.
[0034] Preferably, the pressure after decompression in S4 is 0.4-0.8 Mpa.
[0035] Preferably, the temperature in S4 is raised to 320-360 °C.
[0036] Preferably, the reaction time of S4 is 2 to 4 h.
[0037] The beneficial effects of the present invention are:
[0038] The bio-based degradable nylon of the present invention has good degradation performance, excellent mechanical properties and heat resistance, low water absorption, high yield and molecular weight, excellent comprehensive performance, can be mass-produced, and has good application prospects.
[0039] The bio-based degradable nylon of the invention is prepared by polymerization reaction of biodegradable diamine and dibasic acid as raw materials. The preparation method is green and environmentally friendly, has high economic benefits, is easy to operate, and is conducive to sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a Fourier infrared spectrum characterization diagram of the bio-based degradable nylon prepared in Example 2. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to better understand the technical solution of the invention, the present invention is further described in detail below in conjunction with specific implementation methods.
[0042] Example 1
[0043] This embodiment provides a method for preparing bio-based degradable nylon, the steps are as follows:
[0044] S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 93.7 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:0.6), 0.7 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 205.3 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N2 to replace the air in the reactor;
[0045] S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 360 r / min, heat the reactor to 150 °C and then stop heating, inflate and pressurize to 0.7 MPa, and carry out condensation reaction for 2.5 h to obtain reactant 1;
[0046] S3, raising the temperature of the magnetically driven high-pressure reactor to 290 °C at a rate of 30 °C / min, and setting the pressure of the reactor to 3 MPa. After reaching the temperature, react for 1 h to obtain reactant 2;
[0047] S4, release the pressure to 0.5 MPa, raise the temperature to 340 °C, and vacuum the reaction for 2 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-1).
[0048] The structural formula of the obtained bio-based degradable nylon is:
[0049] .
[0050] Example 2
[0051] S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 156.1 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:1), 0.8 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 242.7 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N2 to replace the air in the reactor;
[0052] The steps of S2 to S4 are the same as those in Example 1, and bio-based degradable nylon (PA-SF-2) is obtained.
[0053] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0054] Example 3
[0055] S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 187.3 g of 2,5-furandicarboxylic acid (the molar ratio of 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:1.2), 0.9 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) and 261.4 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N2 to replace the air in the reactor;
[0056] The steps of S2 to S4 are the same as those in Example 1, and bio-based degradable nylon (PA-SF-3) is obtained.
[0057] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0058] Example 4
[0059] The step of S1 is the same as that of Example 1;
[0060] S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 300 r / min, heat the reactor to 140 °C and then stop heating, inflate and pressurize to 0.5 MPa, and carry out condensation reaction for 2 h to obtain reactant 1;
[0061] S3, raising the temperature of the magnetically driven high-pressure reactor to 270 °C at a rate of 20 °C / min, and setting the pressure of the reactor to 3 MPa. After reaching the temperature, react for 1 h to obtain reactant 2;
[0062] S4, release the pressure to 0.4 MPa, increase the temperature to 320 °C, and vacuum the reaction for 2 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-4).
[0063] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0064] Example 5
[0065] The step of S1 is the same as that of Example 1;
[0066] S2, start stirring of the magnetically driven high-pressure reactor, set the stirring speed to 400 r / min, heat the reactor to 170 °C and then stop heating, inflate and pressurize to 0.9 MPa, and perform condensation reaction for 4 h to obtain reactant 1;
[0067] S3, raising the temperature of the magnetically driven high-pressure reactor to 310 °C at a rate of 40 °C / min, and setting the pressure of the reactor to 4 MPa. After reaching the temperature, react for 3 h to obtain reactant 2;
[0068] S4, release the pressure to 0.8 MPa, increase the temperature to 360 °C, and vacuum the reaction for 4 h, then pressurize and discharge the material to obtain bio-based degradable nylon (PA-SF-5).
[0069] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0070] Example 6
[0071] Same as Example 1, except that:
[0072] The mass of the deionized water accounts for 50% of the sum of the mass of the degradable diamine and the bio-based dibasic acid;
[0073] The mass of the sodium hypophosphite accounts for 0.15% of the sum of the mass of the degradable diamine and the bio-based dibasic acid;
[0074] Bio-based degradable nylon (PA-SF-6) was obtained.
[0075] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0076] Example 7
[0077] Same as Example 1, except that:
[0078] The mass of the deionized water accounts for 70% of the sum of the mass of the degradable diamine and the bio-based dibasic acid;
[0079] The mass of the sodium hypophosphite accounts for 0.31% of the sum of the mass of the degradable diamine and the bio-based dibasic acid;
[0080] Bio-based degradable nylon (PA-SF-7) was obtained.
[0081] The structural formula of the obtained bio-based degradable nylon is the same as that of Example 1.
[0082] Comparative Example 1
[0083] S1. Add 136.2 g p-phenylenediamine, 156.1 g 2,5-furandicarboxylic acid (the molar ratio of p-phenylenediamine to 2,5-furandicarboxylic acid is 1:1), 0.6 g sodium hypophosphite (0.2% of the sum of the mass of p-phenylenediamine and 2,5-furandicarboxylic acid) and 175.4 g deionized water (60% of the sum of the mass of p-phenylenediamine and 2,5-furandicarboxylic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N2 to replace the air in the reactor;
[0084] The steps of S2 to S4 are the same as those of Example 1 to obtain nylon (PA-1).
[0085] Comparative Example 2
[0086] S1. Add 248.4 g of 4,4'-dithiodiphenylamine, 166.1 g of terephthalic acid (the molar ratio of 4,4'-dithiodiphenylamine to terephthalic acid is 1:1), 0.8 g of sodium hypophosphite (0.2% of the sum of the mass of 4,4'-dithiodiphenylamine and terephthalic acid) and 248.7 g of deionized water (60% of the sum of the mass of 4,4'-dithiodiphenylamine and terephthalic acid) into a magnetically driven high-pressure reactor, and introduce a protective atmosphere of N2 to replace the air in the reactor;
[0087] The steps of S2 to S4 are the same as those of Example 1 to obtain nylon (PA-2).
[0088] Effect Example 1 Fourier Infrared Spectroscopy Characterization
[0089] The biodegradable nylon (PA-SF-2) prepared in Example 2 was characterized by infrared spectroscopy. Figure 1 .
[0090] Depend on Figure 1 It can be seen that among them, 3407 cm -1 The characteristic peaks near 2940 cm-1 are attributed to the NH stretching vibration absorption peak on polyamide, while the peak at 2940 cm-1 is -1 The characteristic peaks near 1638 cm-1 are attributed to the antisymmetric and symmetric stretching vibrations of CH on polyamide (amide band I). -1 The characteristic peak at 1106 cm-1 is attributed to the -CO-NH- bending vibration of polyamide (amide band II). -1 The characteristic peaks nearby correspond to the stretching vibration peaks of SS.
[0091] Effect Example 2 Nylon Degradation Performance Test
[0092] The degradation performance of the nylon prepared in the examples and comparative examples was tested, and the results are shown in Table 1.
[0093] Table 1 Degradation performance test results of Comparative Examples 1-2 and Examples 1-7
[0094]
[0095] It can be seen from Table 1 that the weight loss rate of the bio-based degradable nylon prepared in the embodiment of the present invention is relatively high, which reflects the excellent degradation performance of the bio-based degradable nylon of the present invention. However, in Comparative Examples 1 and 2, which do not use the raw materials of the present invention, the weight loss rate is significantly reduced and the degradation performance is significantly deteriorated.
[0096] Effect Example 3 Nylon Mechanical Properties Test
[0097] The mechanical properties of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 2.
[0098] Table 2 Mechanical properties test results of comparative examples 1-2 and embodiments 1-7
[0099]
[0100] It can be seen from Table 2 that the bio-based degradable nylon prepared in the embodiment of the present invention has a higher tensile strength, which reflects the excellent mechanical properties of the bio-based degradable nylon of the present invention. However, Comparative Examples 1 and 2, which do not use the raw materials of the present invention, have lower tensile strength and poorer mechanical properties.
[0101] Effect Example 4 Nylon Thermal Performance Test
[0102] The bio-based degradable nylon prepared in the examples and comparative examples was tested for thermal properties. The results are shown in Table 3.
[0103] Table 3 Thermal performance test results of Comparative Examples 1-2 and Examples 1-7
[0104]
[0105] It can be seen from Table 3 that the bio-based degradable nylon prepared in the embodiment of the present invention has T d5% and T g The value is relatively high, which reflects the excellent thermal properties of the bio-based degradable nylon of the present invention, while Comparative Examples 1 and Comparative Examples 2 which do not use the raw materials of the present invention, T d5% and T g The lower the value, the poorer the mechanical properties.
[0106] Effect Example 5 Nylon water absorption performance test
[0107] The water absorption performance of the nylon prepared in the embodiment and the comparative example was tested, and the results are shown in Table 4.
[0108] Table 4 Water absorption test results of Comparative Examples 1-2 and Examples 1-7
[0109]
[0110] It can be seen from Table 4 that the water absorption rate of the bio-based degradable nylon prepared in the embodiment of the present invention is relatively low, indicating that the bio-based degradable nylon of the present invention is not easy to absorb water, while the comparative examples 1 and 2 which do not use the raw materials of the present invention have relatively high water absorption rates.
[0111] Effect Example 6 Nylon Yield and Molecular Weight Test
[0112] The yield and molecular weight of the nylon prepared in the examples and comparative examples were tested, and the results are shown in Table 5.
[0113] Table 5 Yield and molecular weight test results of Comparative Examples 1-2 and Examples 1-7
[0114]
[0115] It can be seen from Table 5 that the yield and molecular weight of the bio-based degradable nylon prepared in the embodiment of the present invention are both high, and higher than those of the nylon prepared in the comparative example.
[0116] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A bio-based degradable nylon, characterized in that: The raw materials for preparing the method are 4,4'-dithiodiphenylamine and 2,5-furandicarboxylic acid.
2. The bio-based degradable nylon according to claim 1, characterized in that: The molar ratio of the 4,4'-dithiodiphenylamine to 2,5-furandicarboxylic acid is 1:(0.6-1.2).
3. A method for preparing bio-based degradable nylon, characterized in that: The following steps are involved: S1, mixing 4,4'-dithiodiphenylamine, 2,5-furandicarboxylic acid and a solvent in a protective atmosphere to obtain a mixture; S2, stirring the mixture under elevated temperature, stopping the temperature increase after reaching the target temperature and pressurizing to carry out condensation reaction to obtain reactant 1; S3, subjecting the reactant 1 to a reaction after gradually increasing the temperature under a pressurized environment to obtain a reactant 2; S4, releasing the pressure of the reactant 2, raising the temperature, and reacting in a vacuum environment to obtain bio-based degradable nylon.
4. The preparation method according to claim 3, characterized in that: A catalyst is also added to the S1.
5. The preparation method according to claim 4, characterized in that: The catalyst is selected from at least one of sodium hypophosphite, potassium hypophosphite, calcium hypophosphite, phosphate ester, propyl titanate, and boric acid.
6. The preparation method according to claim 3, characterized in that The stirring speed in S2 is 300-400 r / min, and the target temperature is 140-170 °C.
7. The preparation method according to claim 3, characterized in that: The conditions for the gradient heating in S3 are: heating to 270-310°C at a heating rate of 20-40°C / min.
8. The preparation method according to claim 3, characterized in that The pressure after decompression in S4 is 0.4-0.8 MPa.
9. The preparation method according to claim 3, characterized in that: In the S4, the temperature is raised to 320-360°C.