High-light-transmittance aromatic imide film

By heating a specific combination of polymers to be imidized in an air atmosphere, the problem of anaerobic conditions required for the synthesis of aromatic imide films is solved, and an aromatic imide film with high light transmittance and excellent optical properties is achieved, which is suitable for optical applications. and optoelectronics.

CN118772406APending Publication Date: 2024-10-15NINGBO BOYA POLY ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411020048.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-12-05
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The synthesis of existing aromatic imide films requires anaerobic conditions and has limited optical properties, which limits its application in the fields of optics and optoelectronics.

Method used

Using 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxybisphthalene Acid anhydride and N,N-dimethylacetamide are polymerized at a specific molar ratio, and imidized by heating in an air atmosphere to form an aromatic imide film with high light transmittance.

Benefits of technology

The imidization process is realized in an air atmosphere, which reduces the harshness of the process conditions and obtains high light transmittance and excellent optical properties. The light transmittance is not less than 89.6%, the Y value is not greater than 1.67, and the Young's modulus Below 2.45GPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004966947900000121
    Figure BDA0004966947900000121
  • Figure BDA0004966947900000131
    Figure BDA0004966947900000131
Patent Text Reader

Abstract

The invention belongs to the technical field of high polymer materials and synthesis methods thereof, and particularly relates to a high-light-transmittance aromatic imide film which is prepared by the following steps: reacting diamine containing two six-membered rings and dianhydride containing at least two benzene rings in a non-protonated polar solvent to obtain polyamide acid slurry; and forming a film from the polyamide acid slurry by a coating or casting method, and then heating and imidizing in an air atmosphere to obtain the aromatic imide film. The aromatic imide film provided by the invention has the advantages of good colorless transparent performance, excellent optical performance and low Young modulus, can realize the imidization process in the air atmosphere, greatly reduces the process conditions of molding processing, and can realize continuous casting and stretching production.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the parent application is 202211549796.7, the application date is December 5, 2022, and the name of the invention is “A kind of aromatic imide film”. Technical Field

[0002] The present invention belongs to the technical field of polymer materials and synthesis methods thereof. Specifically, the present invention relates to a high light transmittance aromatic imide film. Background Art

[0003] Imide refers to a class of polymers containing an imide ring in the main chain structure. Polyimide has received widespread attention and rapid development due to its excellent comprehensive performance. The synthesis of imide is simple and convenient, and there are multiple synthetic pathways. Its molecular structure and synthesis scheme can be designed according to needs. The processing methods of imide materials are diverse, and they can be used in resins or composite materials in various forms such as prepolymers, cured films, powders, etc. according to material requirements.

[0004] The performance of imide materials usually depends on the selection of synthetic monomers and their proportions, the selection of reaction conditions, etc. From the perspective of monomer selection, the known imide products on the market are usually obtained from chain aliphatic diamines or cyclic aliphatic diamines and aliphatic dianhydrides / aromatic dianhydrides; or from aromatic diamines and aliphatic dianhydrides / aromatic dianhydrides. However, aromatic polyimides will form strong coloring due to the existence of electronic conjugation, intermolecular and intramolecular charge transfer complexes (CTCs). The resulting products are usually yellow or light yellow, with limited optical properties, which hinders their application in the fields of optics and optoelectronics. From the perspective of polymerization reaction conditions, the environmental conditions are demanding, and the imidization process needs to be carried out under anaerobic conditions. Summary of the invention

[0005] In order to overcome the defects in the prior art of synthesizing aromatic imide films, which require harsh imidization conditions and need to be carried out under anaerobic conditions, and the optical properties of the obtained aromatic imide films are limited, a high-transmittance aromatic imide film is provided.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A high-transmittance aromatic imide film, the preparation of which comprises the following steps:

[0008] 1) mixing 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride and N,N-dimethylacetamide and reacting them to obtain a polyamic acid slurry;

[0009] 2) forming a film by coating the polyamic acid slurry, and then heating it in an air atmosphere for imidization to obtain the aromatic imide film;

[0010] The molar ratio of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 4,4'-oxydiphthalic anhydride is 0.03:0.015:0.015.

[0011] Preferably, the reaction temperature in step 1) is 10° C. and the reaction time is 24 h.

[0012] Preferably, the total mass fraction of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride and 4,4'-oxydiphthalic anhydride in the mixed solution after the 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride and N,N-dimethylacetamide is 24.6%;

[0013] The viscosity of the polyamic acid slurry is 28500cp.

[0014] Preferably, step 1) is carried out under a nitrogen atmosphere.

[0015] Preferably, after the reaction in step 1) is completed, the method further comprises filtering and defoaming the polyamic acid slurry.

[0016] Preferably, in step 2), the heating temperature is 270° C., the holding time is 2 h, and the heating rate is 10° C. / min.

[0017] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention relates to an aromatic imide film, wherein an alicyclic diamine containing two six-membered rings and an aromatic tetracarboxylic dianhydride containing at least two benzene rings with specific substituents are selected as polymerization monomers, and bulky alkyl, carboxyl and other substituents are introduced into the diamine monomers, and the alicyclic structure destroys the electronic conjugation, thereby inhibiting the formation of charge transfer complexes between and within imide molecules, improving the optical properties of the polyimide film, and forming a colorless and highly transparent polyimide with a light transmittance of not less than 89.6% and a Y value of not more than 1.67, and the Young's modulus of the obtained polyimide film is below 2.45 GPa. Moreover, the imidization process can be realized in an air atmosphere, and compared with the anaerobic oven conditions with strict oxygen content requirements in the prior art, the method of the present invention greatly reduces the process conditions of the molding process, and can realize continuous cast stretching production.

[0019] When the dianhydride in the present invention is polymerized with the diamine, it improves the optical properties of the polyimide film and further contributes to reducing the Young's modulus.

[0020] The present invention controls the polymerization reaction temperature within the range of 0-20°C, more preferably 5-15°C, and the obtained polyamic acid slurry precursor can be further processed to obtain an aromatic imide film with excellent optical properties; and the reaction conditions are mild, high temperature is not required, and energy consumption is saved. DETAILED DESCRIPTION

[0021] The present invention is further described in detail in the following specific examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0022] Test method:

[0023] Viscosity test method of polyamic acid slurry:

[0024] The polyamic acid slurry obtained in the examples or comparative examples was measured for logarithmic viscosity at 25° C. using a Cannon-Fenske viscometer. The logarithmic viscosity (μ) was calculated by the following formula.

[0025] μ=ln(t s / t0) / C

[0026] t0: reaction solvent circulation time;

[0027] t s : Slurry circulation time;

[0028] C: 0.5 g / dL.

[0029] Light transmittance test method:

[0030] The total light transmittance of the film was measured in the entire wavelength range of 400-700 nm using a spectrophotometer (Nippon Denshoku Industries Co., Ltd., COH-400) and the unit is percentage (%).

[0031] Y value (YI) test method:

[0032] The yellowness (Yellow Index: YI value) of the aromatic imide film obtained in the examples and comparative examples was measured using a UV-visible near-infrared spectrophotometer "V-670" manufactured by JASCO Corporation. After background measurement without a sample, the aromatic imide film was placed on a sample holder, and the transmittance relative to light of 300 to 800 nm was measured to obtain the tristimulus values ​​(X, Y, Z). The YI value was calculated based on the following formula:

[0033] YI=100×(1.2769X-1.0592Z) / Y.

[0034] Young's modulus test method:

[0035] The tensile Young's modulus of the aromatic imide films obtained in Examples and Comparative Examples was measured by a tensile test using an electromechanical universal testing machine (manufactured by INSTRON) at a test speed of 5 m / min and a load cell of 500 N in accordance with JIS K7127.

[0036] Example 1

[0037] An aromatic imide film, the preparation of which comprises the following steps:

[0038] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 6.3111 g of 4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 51.48 g of anhydrous N,N-dimethylacetamide (DMAc) (0.59 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution at a stirring speed of 250 rpm; the temperature of the first solution was adjusted to 10° C., and 4.4133 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (0.0 15mol) and 4.6533g of 4,4'-oxydiphthalic anhydride (0.015mol) are added to the first solution to obtain a mixed solution, wherein the total mass fraction of the dianhydride monomer and the diamine monomer in the mixed solution is 23%; the mixed solution is reacted at 10°C for 24h and then the stirring is stopped to obtain a polyamic acid slurry; the polyamic acid slurry is filtered under reduced pressure, and the filtrate obtained by filtration is vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry, and the viscosity of the slurry is 78000cp.

[0039] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0040] Example 2

[0041] An aromatic imide film, the preparation of which comprises the following steps:

[0042] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 7.1544 g of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 49.71 g of anhydrous N,N-dimethylacetamide (DMAc) (0.57 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution at a stirring speed of 250 rpm; the temperature of the first solution was adjusted to 10°C; 4.4133 g of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane was uniformly added within 30 minutes. ,4,4'-biphenyltetracarboxylic dianhydride (0.015 mol) and 4.6533 g of 4,4'-oxydiphthalic anhydride (0.015 mol) were added to the first solution to obtain a mixed solution, in which the total mass fraction of dianhydride monomer and diamine monomer was 24.6%; the mixed solution was reacted at 10°C for 24 hours, and the stirring was stopped to obtain a polyamic acid slurry; the polyamic acid slurry was filtered under reduced pressure, and the filtrate obtained by filtration was vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry with a viscosity of 28500cp.

[0043] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0044] Example 3

[0045] An aromatic imide film, the preparation of which comprises the following steps:

[0046] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 6.3111 g of 4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 51.55 g of anhydrous N,N-dimethylacetamide (DMAc) (0.59 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution, and the stirring speed was 250 rpm; the temperature of the first solution was adjusted to 10°C, and then 3.9422 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (0.01 mol) and 6.2044 g of 4,4'-oxydiphthalic anhydride (0.02 mol) are added to the first solution until the dianhydride is fully dissolved to obtain a mixed solution, wherein the total mass fraction of the dianhydride monomer and the diamine monomer in the mixed solution is 24.2%; the mixture is reacted at 10°C for 24 hours, and stirring is stopped to obtain a polyamic acid slurry; the polyamic acid slurry is filtered under reduced pressure, and the filtrate obtained by filtration is vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry, and the viscosity of the slurry is 59200cp.

[0047] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0048] Example 4

[0049] 1) Preparation of polyamic acid slurry: Preparation of polyamic acid slurry: Under nitrogen protection, 6.3111 g of 4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 47.14 g of anhydrous N,N-dimethylacetamide (DMAc) (0.54 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution at a stirring speed of 250 rpm; the temperature of the first solution was adjusted to 10°C, and then 5.8844 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (0.02 mol) and 3.1022 g of 4,4'-oxydiphthalic anhydride (0.01 mol) are added to the first solution until the dianhydride is fully dissolved to obtain a mixed solution, in which the total mass fraction of the dianhydride monomer and the diamine monomer is 24.5%; the mixed solution is reacted at 10°C for 24 hours, and stirring is stopped to obtain a polyamic acid slurry; the polyamic acid slurry is filtered under reduced pressure, and the filtrate obtained by filtration is vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry with a viscosity of 64000cp.

[0050] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0051] Example 5

[0052] An aromatic imide film, the preparation of which comprises the following steps:

[0053] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 6.3111 g of 4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 51.48 g of anhydrous N,N-dimethylacetamide (DMAc) (0.59 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution, and the stirring speed was 250 rpm; the temperature of the first solution was adjusted to 10° C., and 8.8266 g of 3,3',4,4'-biphenyltetracarboxylic dianhydride (0.03 mol) was evenly added to the first solution within 30 minutes until the dianhydride was fully dissolved to obtain a mixed solution; the mixed solution was reacted at 10° C. for 24 hours and then the stirring was stopped to obtain a polyamic acid slurry; the polyamic acid slurry was filtered under reduced pressure, and the filtrate obtained by filtration was vacuum defoamed to obtain a viscous and uniform polyamic acid slurry, and the viscosity of the slurry was 45000 cp.

[0054] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0055] Comparative Example 1

[0056] An aromatic imide film, the preparation of which comprises the following steps:

[0057] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 6.3111 g of 4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 43.03 g of anhydrous N,N-dimethylacetamide (DMAc) (0.49 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution, and the stirring speed was 250 rpm; the temperature of the first solution was adjusted to 10° C., and then 6.5436 g of pyromellitic dianhydride (0.03 mol) was uniformly added to the first solution within 30 minutes to obtain a mixed solution; the mixed solution was reacted at 25° C. for 24 hours, and stirring was stopped to obtain a polyamic acid slurry; the polyamic acid slurry was filtered under reduced pressure, and the filtrate obtained by filtration was vacuum defoamed to obtain a viscous and uniform polyamic acid slurry.

[0058] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0059] Comparative Example 2

[0060] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 7.1526 g of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 41.98 g of anhydrous dimethylacetamide (DMAc) (0.48 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution, and the stirring speed was 250 rpm;

[0061] The temperature of the first solution was adjusted to 10°C, and then 6.5436 g of pyromellitic dianhydride (0.03 mol) was evenly added to the first solution within 30 minutes until the dianhydride was fully dissolved to obtain a mixed solution; the mixed solution was reacted at 10°C for 24 hours, and stirring was stopped to obtain polyamic acid slurry; the polyamic acid slurry was filtered under reduced pressure, and the filtrate obtained by filtration was vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry.

[0062] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0063] Comparative Example 3

[0064] An aromatic imide film, the preparation of which comprises the following steps:

[0065] 1) Preparation of polyamic acid slurry: Under nitrogen protection, 3.4256 g of 1,2-diaminocyclohexane (0.03 mol) was added to a 250 mL three-necked flask equipped with a mechanical stirrer; 41.82 g of anhydrous N,N-dimethylacetamide (DMAc) (0.48 mol) was added to the three-necked flask and stirred until the diamine was completely dissolved to obtain a first solution, and the stirring speed was 250 rpm; the temperature of the first solution was adjusted to 10°C, and 4 .4133g of 3,3',4,4'-biphenyltetracarboxylic anhydride (0.015mol) and 4.6533g of 4,4'-oxydiphthalic anhydride (0.015mol) were added to the first solution until the anhydride was fully dissolved to obtain a mixed solution; the mixed solution was reacted at 10°C for 24h and then stirring was stopped to obtain polyamic acid slurry; the polyamic acid slurry was filtered under reduced pressure, and the filtrate obtained by filtration was vacuumized and defoamed to obtain a viscous and uniform polyamic acid slurry.

[0066] 2) Preparation of aromatic imide film: Scrape the viscous and uniform polyamic acid slurry onto a glass plate with an area of ​​25 cm×25 cm to form a film; heat the film-forming polyamic acid slurry to 270°C at a heating rate of 10°C / min in an air atmosphere and keep it warm for 2 hours; cool to room temperature to obtain a 25 μm thick aromatic imide film.

[0067] Test Case

[0068] The light transmittance, Y value and Young's modulus of the aromatic imide films obtained in the above examples and comparative examples were tested according to the above test methods. The test results are shown in Table 1.

[0069] Table 1. Test results

[0070]

[0071]

[0072] The aromatic imide films of Comparative Examples 1-3 have a lower transmittance (88.6-89.1%), a higher Y value (not less than 2.91), and a higher Young's modulus (not less than 3.2 GPa), while the aromatic imide films of Examples 1-5 have a higher transmittance (greater than or equal to 89.6%), a lower Y value (lower than 1.67), high colorlessness and transparency, excellent optical properties, and a lower Young's modulus (lower than 2.45 GPa).

[0073] In summary, the colorless and highly transparent aromatic imide film obtained by using the specific combination of diamine and dianhydride of the present invention exhibits excellent optical properties and a low Young's modulus, and the imidization process can be achieved in an air atmosphere.

[0074] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A high light transmittance aromatic imide film, characterized in that: The preparation of the high-transmittance aromatic imide film comprises the following steps: 1) mixing 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride and N,N-dimethylacetamide and reacting them to obtain a polyamic acid slurry; 2) forming a film by coating the polyamic acid slurry, and then heating it in an air atmosphere for imidization to obtain the aromatic imide film; The molar ratio of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, and 4,4'-oxydiphthalic anhydride is 0.03:0.015:0.

015.

2. The high light transmittance aromatic imide film according to claim 1, characterized in that: The reaction temperature in step 1) is 10° C. and the reaction time is 24 h.

3. The high light transmittance aromatic imide film according to claim 1, characterized in that: The total mass fraction of 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-oxydiphthalic anhydride and N,N-dimethylacetamide in the mixed solution is 24.6%; The viscosity of the polyamic acid slurry is 28500cp.

4. The high light transmittance aromatic imide film according to claim 1, characterized in that: Step 1) was carried out under a nitrogen atmosphere.

5. The high light transmittance aromatic imide film according to claim 1, characterized in that: Step 1) After the reaction is completed, the method further includes filtering and defoaming the polyamic acid slurry.

6. The high light transmittance aromatic imide film according to claim 1, characterized in that: The heating temperature in step 2) is 270°C, the holding time is 2h, and the heating rate is 10°C / min.