Vibration attenuation damping material based on polylipoic acid and copolymer thereof and preparation method of vibration attenuation damping material
By developing vibration damping materials based on polylipoic acid and its copolymers and using chemical and physical cross-linking technology, the problem of underutilized performance of polylipoic acid in the application of vibration damping materials has been solved, achieving high tan δ value, Material preparation with excellent performance, suitable for applications in different temperature ranges.
Patent Information
- Application Number
- CN202410985345.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There is a lack of research and application of polylipoic acid as a vibration damping material in the existing technology, resulting in its performance in vibration and noise control not being fully utilized.
Develop vibration damping materials based on polylipoic acid and its copolymers, prepare them through chemical and physical cross-linking methods, adjust the molecular weight and styrene molar content, and optimize the tan δ value and optimal service temperature to improve the damping performance of the material.
Vibration damping materials with tan δ values close to or greater than 2.0 have been obtained, which have excellent vibration suppression and noise reduction properties. Different types of materials can be obtained by adjusting the molecular weight and ratio to adapt to application requirements in different temperature ranges.
Smart Images

Figure CN118772408A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a damping material, in particular to a damping material based on polythioctic acid and having high loss factor performance. Background Art
[0002] Vibration damping materials are materials that dissipate the mechanical vibration energy of solids into heat energy and are mainly used for vibration and noise control. The damping performance of a material can be measured by its ability to dissipate vibration energy, and the standard for evaluating the damping size is the damping coefficient.
[0003] Vibration damping materials are commonly used in the fields of automobiles, construction, aerospace, and mechanical equipment to improve the performance and stability of the system. Common damping materials include rubber, foam, plastic, metal, and composite materials.
[0004] Rubber and related products prepared by polymer synthesis methods are an important source of shock-absorbing and damping materials. The main indicator for evaluating such materials is the loss factor, which refers to a parameter that indicates the degree of energy loss in a vibration system. The larger the loss factor, the more serious the energy loss of the system. In damping materials, the loss factor can indicate the material's ability to absorb and convert vibration energy. A higher loss factor means that the material has a better vibration suppression effect and can more effectively reduce the spread of vibration and noise. Therefore, when selecting a damping material, its loss factor is usually considered to evaluate its performance.
[0005] The temperature range where the loss factor (tanδ) is greater than 0.3 is the service temperature of the material as a vibration damping material. The larger the tanδ value, the better the vibration damping performance. The temperature corresponding to the maximum tanδ value is the optimal service temperature of the vibration damping material. Currently, the materials with excellent vibration damping performance are mainly rubber and thermoplastic elastomers, and the maximum tanδ value is between 1.5 and 2.
[0006] Polylipoic acid is a very important high molecular polymer material, but there is no research on its application as a vibration damping material in the prior art. Summary of the invention
[0007] In order to solve the problems existing in the above technologies, the present invention provides a vibration damping material based on polylipoic acid with high loss factor performance.
[0008] The present invention provides a vibration reduction and damping material based on polylipoic acid and its copolymer, which comprises:
[0009] The damping material is polylipoic acid;
[0010] Alternatively, the damping material is lipoic acid-styrene copolymer;
[0011] Alternatively, the damping material is a polymer obtained by chemically and physically crosslinking polylipoic acid and lipoic acid-styrene random copolymer;
[0012] The molecular weight of the damping material is greater than 20 kg·mol -1 .
[0013] Preferably, the damping material has a molecular weight of 43.7 kg·mol -1 Polylipoic acid, tanδ maximum value is 2.83, the best service temperature is 15℃, and the service temperature range is -1 to 31℃;
[0014] Alternatively, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 139°C, a maximum tanδ of 2.03, an optimal service temperature of 7°C, and a service temperature range of -20 to 58°C.
[0015] Alternatively, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 154°C, a maximum tanδ of 2.12, an optimal service temperature of 3°C, and a service temperature range of -22 to 48°C.
[0016] Alternatively, the damping material has a molecular weight of 32.1 kg·mol -1 , the maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 50% is 2.98, the optimal service temperature is 25℃, and the service temperature range is -6 to 59℃;
[0017] Alternatively, the damping material has a molecular weight of 40.3 kg·mol -1 , the maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 31% is 2.92, the optimal service temperature is 24℃, and the service temperature range is 10 to 41℃;
[0018] Alternatively, the damping material has a molecular weight of 83.6 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 24%, a viscosity-flow transition temperature of 63°C, a maximum tanδ value of 2.02, an optimal service temperature of 9°C, and a service temperature range of -33 to 43°C.
[0019] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 37%, a viscosity-flow transition temperature of 70°C, a maximum tanδ of 2.43, an optimal service temperature of 27°C, and a service temperature range of 10 to 56°C.
[0020] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 22%, a viscosity-flow transition temperature of 81°C, a maximum tanδ of 2.23, an optimal service temperature of 21°C, and a service temperature range of 3 to 50°C.
[0021] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 16%, a viscosity-flow transition temperature of 72°C, a maximum tanδ of 2.29, an optimal service temperature of 21°C, and a service temperature range of 4 to 52°C.
[0022] Preferably, the crosslinking agent used in the chemical crosslinking method includes: at least one of polyols, polyisocyanates, polyglycidyl ethers, polyacids such as citric acid, 2,3-dihydroxysuccinic acid (tartaric acid), tannic acid (tannic acid), catechol (catechol), resorcinol, hydroquinone (hydroquinone), phloroglucinol, bisphenol A (BPA), metal salts and carbonyl diimidazole compounds, or a combination thereof.
[0023] Preferably, the polylipoic acid is cross-linked polylipoic acid, and the synthetic formula of the cross-linked polylipoic acid is Figure 1 The polylipoic acid copolymer is a cross-linked lipoic acid-styrene random copolymer, and the synthesis method of the cross-linked lipoic acid-styrene random copolymer is the same as that of the cross-linked polylipoic acid, and only the polymer substrate needs to be replaced from polylipoic acid to lipoic acid-styrene random copolymer.
[0024] The present invention provides a method for preparing a vibration damping material based on polylipoic acid and its copolymer, which comprises the following steps:
[0025] The lipoic acid monomer is added with an initiator in a solvent 1 to carry out a ring-opening polymerization reaction, and a terminator is added after the reaction to obtain polylipoic acid;
[0026] The molar ratio of lipoic acid to initiator is 5000:(1-100), stirring at low temperature or room temperature for 30min-4h, adding pre-cooled propyl mercaptan to terminate the polymerization reaction, removing the initiator residue, and waiting for the solvent to evaporate completely;
[0027] The initiator is first dissolved in solvent 2 and mixed evenly before being added into solvent 1;
[0028] The solvent one and solvent two are respectively selected from at least one of methyl chloride, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, n-hexane, cyclohexane, n-heptane, tetrahydrofuran, acetone, butanone, ether, acetonitrile, benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.
[0029] Preferably, the method comprises the following steps:
[0030] Add lipoic acid monomer and styrene monomer into the solvent, and then add initiator to react;
[0031] After the reaction, a reaction terminator is added to obtain a lipoic acid-styrene random copolymer;
[0032] Drying the random copolymer of styrene and lipoic acid to obtain a damping material;
[0033] Preferably, the method comprises the following steps:
[0034] The initiator is first dissolved in a solvent to form an initiator solution and then mixed with the reaction monomer;
[0035] The reaction terminator is deionized water or an alkyl alcohol solution or a mercaptan solution;
[0036] The molar ratio of lipoic acid monomer to styrene monomer is 10:1 to 1:10; the molar ratio of the amount of initiator to the total amount of monomers is 1:1000 to 1:100; the concentration of the reaction monomer solution is 0.01 to 1 mol / L, and the mixture is stirred at low or normal temperature for 5 minutes to 4 hours;
[0037] The solvent used is at least one of methyl chloride, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, n-hexane, cyclohexane, n-heptane, tetrahydrofuran, acetone, butanone, ether, acetonitrile, benzonitrile, benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, and butyl sulfone.
[0038] The initiator is one of the following substances: trifluoromethanesulfonic acid, trifluoromethanesulfonic anhydride, methyl trifluoromethanesulfonate, ethyl trifluoromethanesulfonate, butyl trifluoromethanesulfonate, allyl trifluoromethanesulfonate, benzyl trifluoromethanesulfonate, o-tolyl trifluoromethanesulfonate, 4-biphenyl trifluoromethanesulfonate, trifluoroacetic acid;
[0039] The initiator is a two-component agent, and the initiator in the two-component initiation system is selected from at least one of allyl chloride, allyl bromide, methylallyl chloride, methylallyl bromide, benzyl chloride, benzyl bromide, α,α-dimethylbenzyl chloride, α,α-dimethylbenzyl bromide, 1,3-di(chloromethyl)benzene, 1,3-di(bromomethyl)benzene, 1,4-di(chloromethyl)benzene, 1,4-di(bromomethyl)benzene, 1,3,5-tri(chloromethyl)benzene, and 1,3,5-tri(bromomethyl)benzene.
[0040] The initiator is a two-component agent, and the co-initiator in the two-component initiation system is selected from silver fluorosulfonate, silver trifluoromethanesulfonate, trifluoromethanesulfonates of lanthanide elements (yttrium, scandium, dysprosium, samarium, gadolinium and neodymium), silver hexafluorophosphate, silver hexafluoroarsenate, silver hexafluoroantimonate, lithium perchlorate, potassium perchlorate, manganese perchlorate, silver perchlorate, magnesium perchlorate, calcium perchlorate, cesium perchlorate, barium perchlorate, iron perchlorate and the like, zinc dichloride, cadmium dichloride, mercuric dichloride, aluminum trichloride, aluminum tribromide, gallium trichloride, iron trichloride, tin tetrachloride, titanium tetrachloride, zirconium tetrachloride, vanadium tetrachloride, antimony pentafluoride, antimony pentachloride, antimony hexafluoride, tungsten pentachloride, boron trichloride, boron trifluoride, boron tribromide, AlR m X 3-m (R is an alkyl group such as methyl or ethyl, and X is a halogen) or the like.
[0041] Beneficial effects of the present invention:
[0042] 1. The present invention synthesizes different types of vibration damping materials based on polylipoic acid, wherein the tanδ values of these vibration damping materials based on polylipoic acid are close to 2.0 or greater than 2.0, and the vibration damping materials obtained from some polymers have better performance, which indicates that the present invention obtains vibration damping materials based on polylipoic acid with excellent performance;
[0043] 2. By adjusting the ratio of lipoic acid-styrene copolymer, vibration damping materials with different properties are obtained accordingly. Specifically, the molecular weight is 32.1 kg·mol -1 The maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 50% is 2.98, the optimal service temperature is 25℃, and the service temperature range is -6 to 59℃; the molecular weight is 40.3kg·mol -1 The maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 31% is 2.92, the optimal service temperature is 24℃, and the service temperature range is 10 to 41℃; the molecular weight is 83.6kg·mol -1 The maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 24% is 2.02, the optimal service temperature is 9°C, and the service temperature range is -33 to 43°C. By adjusting different molecular weights and proportions, different types of vibration damping materials are obtained, and the most suitable material is selected according to needs. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The present invention is a schematic diagram of molecular synthesis of a polylipoic acid cross-linked damping material prepared by chemical and physical cross-linking methods. DETAILED DESCRIPTION
[0045] Embodiment 1:
[0046] The vibration damping material based on polythioctic acid and its copolymer of this embodiment includes the damping material being polythioctic acid. The damping material is a polymer having a molecular weight of 43.7 kg·mol -1 The maximum value of tanδ of polylipoic acid is 2.83, the optimal service temperature is 15℃, and the service temperature range is -1 to 31℃.
[0047] The present embodiment provides a method for preparing a vibration damping material based on polylipoic acid and its copolymer, which comprises the following steps:
[0048] The lipoic acid monomer is dissolved in solvent 1, an initiator is added to carry out a ring-opening polymerization reaction, and a terminator is added after the reaction to obtain polylipoic acid;
[0049] The molar ratio of lipoic acid to initiator was 200:1. The mixture was stirred at low temperature of 0°C for 2 h, and 0°C pre-cooled propanethiol was added to terminate the polymerization reaction. The initiator residue was removed and the solvent was completely evaporated.
[0050] The initiator is first dissolved in solvent 2 and mixed evenly before being added into solvent 1;
[0051] The solvent one and the solvent two are respectively selected from chloroform.
[0052] Embodiment 2:
[0053] In this embodiment, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 139°C, a maximum tanδ of 2.03, an optimal service temperature of 7°C, and a service temperature range of -20 to 58°C.
[0054] Alternatively, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 154°C, a maximum tanδ of 2.12, an optimal service temperature of 3°C, and a service temperature range of -22 to 48°C.
[0055] The synthesis process of the two polylipoic acids adopts the reaction steps in Example 1, and the molar ratios of lipoic acid to initiator are 1500:1 and 2000:1 respectively.
[0056] Alternatively, the damping material has a molecular weight of 32.1 kg·mol -1 The maximum value of tanδ of the lipoic acid-styrene copolymer with a styrene molar content of 50% is 2.98, the optimal service temperature is 25°C, and the service temperature range is -6 to 59°C; the molecular structure of the synthesized lipoic acid-styrene copolymer is:
[0057]
[0058] Alternatively, the damping material has a molecular weight of 40.3 kg·mol -1 , the maximum value of tanδ of lipoic acid-styrene copolymer with styrene molar content of 31% is 2.92, the optimal service temperature is 24℃, and the service temperature range is 10 to 41℃;
[0059] Alternatively, the damping material has a molecular weight of 83.6 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 24%, a viscosity-flow transition temperature of 63°C, a maximum tanδ value of 2.02, an optimal service temperature of 9°C, and a service temperature range of -33 to 43°C.
[0060] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 37%, a viscosity-flow transition temperature of 70°C, a maximum tanδ of 2.43, an optimal service temperature of 27°C, and a service temperature range of 10 to 56°C.
[0061] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 22%, a viscosity-flow transition temperature of 81°C, a maximum tanδ of 2.23, an optimal service temperature of 21°C, and a service temperature range of 3 to 50°C.
[0062] Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 16%, a viscosity-flow transition temperature of 72°C, a maximum tanδ of 2.29, an optimal service temperature of 21°C, and a service temperature range of 4 to 52°C.
[0063] The preparation method of the lipoic acid-styrene copolymer of the present embodiment comprises the following steps:
[0064] Adding lipoic acid monomer and styrene monomer into a solvent (adding a specific amount of monomers according to different molar ratios of lipoic acid monomer and styrene monomer), and then adding an initiator to react;
[0065] After the reaction, a reaction terminator is added to obtain a lipoic acid-styrene random copolymer;
[0066] Drying the random copolymer of styrene and lipoic acid to obtain a damping material;
[0067] Preferably, the initiator is first dissolved in a solvent to form an initiator solution and then mixed with the reaction monomer; the reaction terminator is a propylthiol solution; the molar ratio of the initiator amount to the total monomer amount is 1:50; the total concentration of the reaction monomer solution is 1 mol / L, and the mixture is stirred at room temperature for 2 hours;
[0068] The solvent is chloroform;
[0069] The initiator is methyl trifluoromethanesulfonate.
[0070] Embodiment 3:
[0071] The crosslinking agent used in the chemical crosslinking method of this embodiment includes: at least one of polyols, polyisocyanates, polyglycidyl ethers, polyacids such as citric acid, 2,3-dihydroxysuccinic acid (tartaric acid), tannic acid (tannic acid), catechol (catechol), resorcinol, hydroquinone (hydroquinone), phloroglucinol, bisphenol A (BPA), metal salts and carbonyl diimidazole compounds, or a combination thereof.
[0072] The polylipoic acid is cross-linked polylipoic acid, and the synthesis formula of the cross-linked polylipoic acid is: Figure 1 .
[0073] The polylipoic acid copolymer is a cross-linked lipoic acid-styrene random copolymer. The synthesis method of the cross-linked lipoic acid-styrene random copolymer is the same as that of the cross-linked polylipoic acid, and only requires changing the polymer substrate from polylipoic acid to lipoic acid-styrene random copolymer.
[0074] Embodiment 4:
[0075] The following specific materials are obtained accordingly, and the corresponding tanδ and service temperature range are obtained through testing. The preferred materials are obtained through analysis of these materials.
[0076] Molecular weight: 81.3 kg·mol -1 The maximum value of tanδ of polylipoic acid is 2.43, the optimal service temperature is 18℃, and the service temperature range is -7 to 56℃; the upper limit of the service temperature of this material is better than the following materials.
[0077] Molecular weight: 81.3 kg·mol -1 The maximum value of tanδ of the material after polylipoic acid is chemically cross-linked by hexanediol (the molar ratio of carboxyl group to cross-linking agent hexanediol is 24:1) is 1.92, the optimal service temperature is 20°C, and the service temperature range is -5 to 44°C;
[0078] Molecular weight: 81.3 kg·mol -1The maximum tanδ of the material after polylipoic acid is chemically cross-linked with hexanediol (the molar ratio of carboxyl to hydroxyl is 32:1) is 1.86, the optimal service temperature is 22°C, and the service temperature range is -3 to 46°C;
[0079] Molecular weight: 81.3 kg·mol -1 The maximum tanδ value of the material after polylipoic acid is chemically cross-linked with hexamethylene diisocyanate (the molar ratio of carboxyl group to isocyanate group is 32:1) is 1.57, the optimal service temperature is 6°C, and the service temperature range is -16 to 46°C; the service temperature of this material can reach -16°C, which has unique advantages.
[0080] Through further mechanical property tests, the invention shows that the mechanical strength is increased by 1-2 times after chemical cross-linking, while still maintaining relatively high damping performance (the maximum value of tan δ is 1.5 to 2).
[0081] In the above reaction process, preferably, the molar ratio of carboxyl groups in polylipoic acid or lipoic acid-styrene copolymer to reactive functional groups in the crosslinking agent is 4:1 to 64:1, the reaction temperature is 25 to 100°C, the solvent is ethanol or acetone or N,N-dimethylformamide, no catalyst is added or one or more of the following catalysts are added: N,N-dicyclohexylcarbodiimide (DCC) or N,N-diisopropylcarbodiimide (DIC) or other group-substituted carbodiimides, 4-dimethylaminopyridine (DMAP), N,N′-carbonyldiimidazole (CDI) or other group-substituted carbonyldiimidazoles, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) or 1,5-diazabicyclo[4.3.0]-5-nonene (DBN), dibutyltin dilaurate (DBTDL), and the reaction time is 2 to 12 hours.
[0082] In the cross-linking reaction carried out in this embodiment, the synthesis process at the upper position is to obtain a cross-linked damping material by cross-linking polythioic acid and OH-R-OH, where R is, for example, a carbon chain of 2 carbons, or a carbon chain of 6 carbons, or other corresponding molecular structures; the synthesis process at the upper left position is to obtain a cross-linked damping material by cross-linking polythioic acid and OCN-R-NCO, where R is, for example, a carbon chain of 6 carbons or other corresponding molecular structures; the synthesis process at the lower left position is to obtain a cross-linked damping material by cross-linking polythioic acid and diglycidyl ether, where R is, for example, a carbon chain of 6 carbons or other corresponding molecular structures; the synthesis process at the lower position is to obtain a cross-linked damping material by cross-linking polythioic acid and polycarboxylic acid; the synthesis process at the lower right position is to obtain a cross-linked damping material by cross-linking polythioic acid and polyphenol; the synthesis process at the upper right position is to obtain a cross-linked damping material by cross-linking polythioic acid and M n+ (X -)n molecules are cross-linked to obtain the corresponding damping material, where M is a metal atom and X is a halogen atom or an acid ion, such as AlCl 3 , CaCl 2 , Al 2 (SO 4 ) 3 ,Mg 2 (SO 4 ) 3 , Zn 2 (SO 4 ) 3 .
Claims
1. A vibration damping material based on polylipoic acid and its copolymer, characterized in that: The damping material is polylipoic acid; Alternatively, the damping material is lipoic acid-styrene copolymer; Alternatively, the damping material is a polymer obtained by chemically and physically crosslinking polylipoic acid and lipoic acid-styrene random copolymer; The molecular weight of the damping material is greater than 20 kg·mol -1 .
2. The vibration damping material based on polylipoic acid and its copolymer according to claim 1, characterized in that: The polylipoic acid-based polymer material in the damping material forms a physical cross-linking network through hydrogen bonds, and forms a chemical cross-linking network and a physical cross-linking network through chemical reactions of carboxyl groups and hydrogen bonds, respectively. The physical and chemical cross-linking networks dissipate a large amount of energy, and the flexible main chain containing sulfur atoms synergistically gives it vibration reduction and damping properties.
3. The vibration damping material based on polylipoic acid and its copolymer according to claim 1, characterized in that: The damping material has a molecular weight of 43.7 kg·mol -1 Polylipoic acid, tanδ maximum value is 2.83, the best service temperature is 15℃, and the service temperature range is -1 to 31℃; Alternatively, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 139°C, a maximum tanδ of 2.03, an optimal service temperature of 7°C, and a service temperature range of -20 to 58°C. Alternatively, the damping material has a molecular weight exceeding 300 kg·mol -1 The polylipoic acid has a viscosity-flow transition temperature of 154°C, a maximum tanδ of 2.12, an optimal service temperature of 3°C, and a service temperature range of -22 to 48°C. Alternatively, the damping material has a molecular weight of 32.1 kg·mol -1 , lipoic acid-styrene copolymer with a styrene molar content of 50%, a maximum tanδ of 2.98, an optimal service temperature of 25°C, and a service temperature range of -6 to 59°C; Alternatively, the damping material has a molecular weight of 40.3 kg·mol -1 , lipoic acid-styrene copolymer with a styrene molar content of 31%, a maximum tanδ of 2.92, an optimal service temperature of 24°C, and a service temperature range of 10 to 41°C; Alternatively, the damping material has a molecular weight of 83.6 kg·mol -1 , lipoic acid-styrene copolymer with a styrene molar content of 24%, a viscosity-flow transition temperature of 63°C, a maximum tanδ of 2.02, an optimal service temperature of 9°C, and a service temperature range of -33 to 43°C; Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , lipoic acid-styrene copolymer with a styrene molar content of 37%, a viscosity-flow transition temperature of 70°C, a maximum tanδ of 2.43, an optimal service temperature of 27°C, and a service temperature range of 10 to 56°C; Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , lipoic acid-styrene copolymer with a styrene molar content of 22%, a viscosity-flow transition temperature of 81°C, a maximum tanδ of 2.23, an optimal service temperature of 21°C, and a service temperature range of 3 to 50°C; Alternatively, the damping material has a relatively high molecular weight exceeding 100 kg·mol -1 , the lipoic acid-styrene copolymer with a styrene molar content of 16%, a viscosity-flow transition temperature of 72°C, a maximum tanδ of 2.29, an optimal service temperature of 21°C, and a service temperature range of 4 to 52°C.
4. The vibration damping material based on polylipoic acid and its copolymer according to claim 1, characterized in that: The crosslinking agents used in the chemical and physical crosslinking methods include: at least one of polyols, polyisocyanates, polyglycidyl ethers, polyacids such as citric acid, 2,3-dihydroxysuccinic acid (tartaric acid), tannic acid (tannic acid), catechol (catechol), resorcinol, hydroquinone (hydroquinone), phloroglucinol, bisphenol A (BPA), metal salts and carbonyl diimidazole compounds, or a combination thereof.
5. The vibration damping material based on polylipoic acid and its copolymer according to claim 4, characterized in that: The polylipoic acid is cross-linked polylipoic acid, and the synthesis formula of the cross-linked polylipoic acid is:
6. The vibration damping material based on polylipoic acid and its copolymer according to claim 4, characterized in that: The polylipoic acid copolymer is a cross-linked lipoic acid-styrene random copolymer. The synthesis method of the cross-linked lipoic acid-styrene random copolymer is the same as that of the cross-linked polylipoic acid, and only requires changing the polymer substrate from polylipoic acid to lipoic acid-styrene random copolymer.
7. The method for preparing a vibration damping material based on polylipoic acid and its copolymer according to claim 1, characterized in that: The following steps are included: The lipoic acid monomer is added with an initiator in a solvent 1 to carry out a ring-opening polymerization reaction, and a terminator is added after the reaction to obtain polylipoic acid; The molar ratio of lipoic acid to initiator is 5000:(1-100), stirring at low temperature or room temperature for 30min-4h, adding propyl mercaptan to terminate the polymerization reaction, removing the initiator residue, and waiting for the solvent to evaporate completely; The initiator is first dissolved in solvent 2 and mixed evenly before being added into solvent 1; The solvent one and solvent two are respectively selected from at least one of methyl chloride, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, n-hexane, cyclohexane, n-heptane, tetrahydrofuran, acetone, butanone, ether, acetonitrile, benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.
8. The method for preparing a vibration damping material based on polylipoic acid and its copolymer according to claim 1, characterized in that: The following steps are included: Add lipoic acid monomer and styrene monomer into the solvent, and then add initiator to react; After the reaction, a reaction terminator is added to obtain a lipoic acid-styrene random copolymer; The random copolymer of styrene and thioctic acid is dried to obtain a damping material.
9. The method for preparing a vibration damping material based on polylipoic acid and its copolymer according to claim 7, characterized in that: The following steps are included: The initiator is first dissolved in a solvent to form an initiator solution and then mixed with the reaction monomer; The reaction terminator is deionized water or an alkyl alcohol solution or a mercaptan solution; The molar ratio of lipoic acid monomer to styrene monomer is 10:1 to 1:10; the molar ratio of the amount of initiator to the total amount of monomers is 1:1000 to 1:100; the concentration of the reaction monomer solution is 0.01 to 1 mol / L, and the mixture is stirred at low or normal temperature for 5 minutes to 4 hours; The solvent used is at least one of methyl chloride, dichloromethane, chloroform, carbon tetrachloride, ethylene dichloride, n-hexane, cyclohexane, n-heptane, tetrahydrofuran, acetone, butanone, ether, acetonitrile, benzonitrile, benzene, toluene, xylene, chlorobenzene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, and butyl sulfone; The initiator is one of the following substances: trifluoromethanesulfonic acid, trifluoromethanesulfonic anhydride, methyl trifluoromethanesulfonate, ethyl trifluoromethanesulfonate, butyl trifluoromethanesulfonate, allyl trifluoromethanesulfonate, benzyl trifluoromethanesulfonate, o-tolyl trifluoromethanesulfonate, 4-biphenyl trifluoromethanesulfonate, trifluoroacetic acid; The initiator is a two-component agent, and the initiator in the two-component initiation system is selected from at least one of allyl chloride, allyl bromide, methylallyl chloride, methylallyl bromide, benzyl chloride, benzyl bromide, α,α-dimethylbenzyl chloride, α,α-dimethylbenzyl bromide, 1,3-di(chloromethyl)benzene, 1,3-di(bromomethyl)benzene, 1,4-di(chloromethyl)benzene, 1,4-di(bromomethyl)benzene, 1,3,5-tri(chloromethyl)benzene, and 1,3,5-tri(bromomethyl)benzene; The initiator is a two-component agent, and the co-initiator in the two-component initiation system is selected from silver fluorosulfonate, silver trifluoromethanesulfonate, trifluoromethanesulfonates of lanthanide elements (yttrium, scandium, dysprosium, samarium, gadolinium and neodymium), silver hexafluorophosphate, silver hexafluoroarsenate, silver hexafluoroantimonate, lithium perchlorate, potassium perchlorate, manganese perchlorate, silver perchlorate, magnesium perchlorate, calcium perchlorate, cesium perchlorate, barium perchlorate, iron perchlorate and the like, zinc dichloride, cadmium dichloride, mercuric dichloride, aluminum trichloride, aluminum tribromide, gallium trichloride, iron trichloride, tin tetrachloride, titanium tetrachloride, zirconium tetrachloride, vanadium tetrachloride, antimony pentafluoride, antimony pentachloride, antimony hexafluoride, tungsten pentachloride, boron trichloride, boron trifluoride, boron tribromide, AlR m X 3-m (R is an alkyl group such as methyl or ethyl, and X is a halogen) or the like.
Citation Information
Patent Citations
Preparation method of polylipoic acid renewable polymer material
CN115490861A
Preparation method of styrene thermoplastic polymer material
CN116396478A
Adhesive as well as preparation method and bonding use method thereof
CN118272038A
Cited By
Hydroxyl ester group-containing polydisulfide high polymer material and preparation method thereof
CN119708491A