A recyclable shape memory composite material based on polyarylethernitrile and having super mechanical properties, and its preparation method and application

By introducing dynamic covalent bonds of polyvinylpyrrolidone and boron oxygen, as well as carboxylic acid groups in polyarylethernitriles, the problem of insufficient mechanical properties and thermal properties of shape memory polymers is solved, and high heat resistance, pressure resistance and resistance are achieved Chemical corrosion performance, recyclable properties, suitable for applications under harsh environmental conditions.

CN118772422BActive Publication Date: 2024-11-29SOUTHWEST PETROLEUM UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411238922.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-29
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Existing shape memory polymers have significant shortcomings in mechanical and thermal properties, limiting their application under harsh environmental conditions and lacking recyclable properties.

Method used

By introducing dynamic covalent bonds of polyvinylpyrrolidone and boron oxygen into the molecular structure of polyarylethernitriles, as well as carboxylic acid groups, nucleophilic aromatic substitution polycondensation reaction and radical polymerization, high heat resistance, pressure resistance and Shape memory composite material with chemical corrosion resistance.

Benefits of technology

It significantly improves the mechanical properties and thermal stability of shape memory polymers, has excellent shape memory effects, and realizes the recyclable properties of materials. It is suitable for harsh environmental conditions and meets the requirements of green environmental protection and sustainable development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772422B_ABST
    Figure CN118772422B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of shape memory of polymer materials, and specifically relates to a recyclable shape memory composite material with super mechanical properties based on polyarylethernitrile, and a preparation method and application thereof. The recyclable shape memory composite polymer material with super mechanical properties prepared by the present invention solves the problem of insufficient mechanical and thermal properties of existing shape memory polymers by introducing polyvinylpyrrolidone and boron oxygen dynamic covalent bonds, as well as carboxylic acid groups into the molecular structure of polyarylethernitrile. The composite polymer material containing the above groups has high heat resistance, pressure resistance and chemical corrosion resistance, and at the same time has excellent shape memory effect, can maintain stable performance under harsh environmental conditions, and has recyclable performance, which meets the requirements of green environmental protection and sustainable development.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of shape memory of polymer materials, and in particular relates to a shape memory composite material based on polyarylethernitrile that is recyclable and has super mechanical properties, and a preparation method and application thereof. Background Art

[0002] Shape memory polymers are a type of smart material that can remember and restore its original shape under specific conditions (such as temperature, light, electric field, magnetic field, etc.). Due to its broad application prospects in aerospace, medical devices, electronic equipment, and smart textiles, shape memory polymers have received widespread attention in recent years.

[0003] Poly(arylether nitrile) is a class of high-performance polymer materials with excellent thermal stability, chemical resistance and high mechanical strength. Due to the rigid aromatic ring and heat-resistant ether bond in its molecular structure, poly(arylether nitrile) exhibits a high glass transition temperature and thermal decomposition temperature. In addition, the mechanical strength and modulus of poly(arylether nitrile) are significantly higher than those of traditional shape memory polymers. However, existing shape memory polymers have significant deficiencies in mechanical and thermal properties, which limits their practical applications.

[0004] In order to overcome the above-mentioned defects, the present invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a recyclable shape memory composite material based on polyarylethernitrile with super mechanical properties, which has high heat resistance, pressure resistance and chemical corrosion resistance, and at the same time has excellent shape memory effect, solving the problem of insufficient mechanical and thermal properties of existing shape memory polymers, and can maintain stable performance under harsh environmental conditions. It also has recyclability and meets the requirements of green environmental protection and sustainable development.

[0006] The second purpose of the present invention is to provide a method for preparing a recyclable shape memory composite material based on poly(arylene ether nitrile) with super mechanical properties. Compared with traditional shape memory polymers, the shape memory polymer material prepared by this method shows significant improvement in thermal properties, especially mechanical properties, and can maintain stable performance under harsh environmental conditions.

[0007] The third object of the present invention is to provide a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties for use in fields including aerospace, medical equipment, electronic equipment or smart textiles.

[0008] The present invention is achieved through the following technical solutions:

[0009] In a first aspect, the present invention provides a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties, wherein the composite material is represented by formula (I):

[0010] Formula (I) ;

[0011] Wherein, n is an integer between 80 and 100, x+y+z=1 and x>0, y>0, z>0; i is an integer between 270 and 3250;

[0012] Wherein, R1 is selected from formula (II) or formula (III);

[0013] The above formula (II) is , wherein m1 is an integer between 20 and 35, and R6 is selected from -H, substituted or unsubstituted C 1-18 A group consisting of an alkyl group;

[0014] The above formula (III) is , where m2 is an integer between 10 and 55;

[0015] Among them, R2 contains a phenylboronic acid structure.

[0016] Furthermore, in a preferred embodiment of the present invention, the above R6 is selected from -H, substituted or unsubstituted C 18 .

[0017] In a second aspect, the present invention provides a method for preparing a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties, comprising the following steps:

[0018] S1. Add bisphenol A, 2,6-dihalobenzonitrile, 2,2-diallylbisphenol A, phenolphthalein and a catalyst into a reaction container, then add a first solvent and a water-carrying agent, mix well and heat to boiling, and reflux to react until all water is removed; continue to heat the reaction system to 170-190° C., keep the temperature for 1-2 hours to obtain a reaction mixture containing polyarylethernitrile, precipitate, filter and dry the reaction mixture to obtain a crude polyarylethernitrile containing a carboxylic acid group;

[0019] S2, dissolving the crude product obtained in step S1 in a first solvent, and then adding concentrated hydrochloric acid to acidify to obtain a poly(arylene ether nitrile) mixture containing carboxylic acid groups, and sequentially precipitating, filtering, purifying, and drying the mixture to obtain a poly(arylene ether nitrile) final product containing carboxylic acid groups;

[0020] S3, dissolving the final product obtained in step S2 in a second solvent, adding monomer 1, monomer 2 and an initiator, stirring and dissolving them, and continuing to heat the reaction system to 60-80° C. and keeping the temperature for 10-14 hours to obtain a shape memory polyarylethernitrile solution;

[0021] S4, uniformly mixing the shape memory poly(arylene ether nitrile) solution prepared in step S3 with a polyvinyl pyrrolidone solution dissolved in a second solvent, and then evaporating the solvent to obtain a recyclable shape memory composite material having super mechanical properties;

[0022] The monomer 1 is selected from olefin compounds containing R1 structure, and the monomer 2 is selected from olefin compounds containing phenylboronic acid structure.

[0023] Furthermore, in a preferred embodiment of the present invention, the above-mentioned monomer 1 is octadecyloxy polyethylene glycol methacrylate, polyethylene glycol methyl acrylate, polyethylene glycol ethyl methacrylate or allyl polyethylene glycol; and the above-mentioned monomer 2 is 3-vinylbenzeneboronic acid, 4-vinylbenzeneboronic acid or acrylamidophenylboronic acid.

[0024] Furthermore, in a preferred embodiment of the present invention, in the above step S1, the sum of the molar quantities of bisphenol A, 2,2-diallylbisphenol A and phenolphthalein is equal to the molar quantity of 2,6-dihalobenzonitrile.

[0025] Furthermore, in a preferred embodiment of the present invention, the first solvent is N-methylpyrrolidone; the water-carrying agent is toluene; the catalyst is anhydrous potassium carbonate, sodium carbonate, potassium hydroxide or sodium hydroxide; the second solvent is N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

[0026] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the polyvinyl pyrrolidone in the above step S4 to the poly(arylene ether nitrile) final product containing carboxylic acid groups obtained in step S2 is 1-20:100.

[0027] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2 added in the above step S3 is 10:1-4:1-4.

[0028] Furthermore, in a preferred embodiment of the present invention, the molar ratio of the catalyst to 2,6-dihalobenzonitrile is 1:1-1.5; and the volume ratio of the water-carrying agent to the first solvent is 1:2-4.

[0029] Furthermore, in a preferred embodiment of the present invention, the mass of the initiator added in the above step S3 accounts for 0.2-2% of the total mass of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2.

[0030] Further preferably, in a preferred embodiment of the present invention, the 2,6-dihalobenzonitrile is selected from 2,6-dichlorobenzonitrile and 2,6-difluorobenzonitrile.

[0031] In a third aspect, the present invention provides a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties for use in fields including aerospace, medical equipment, electronic equipment or smart textiles.

[0032] Compared with the prior art, the present invention has at least the following technical effects:

[0033] 1. The present invention provides a recyclable shape memory composite material with super mechanical properties based on polyarylethernitrile. By introducing polyvinylpyrrolidone and boron oxygen dynamic covalent bonds, as well as carboxylic acid groups into the molecular structure of polyarylethernitrile, the problem of insufficient mechanical and thermal properties of existing shape memory polymers is solved. The composite polymer material containing the above groups has high heat resistance, pressure resistance and chemical corrosion resistance, and at the same time has excellent shape memory effect, can maintain stable performance under harsh environmental conditions, and has recyclable performance, which meets the requirements of green environmental protection and sustainable development.

[0034] 2. The present invention provides a method for preparing a recyclable shape memory composite material with super mechanical properties based on poly(arylether nitrile), wherein poly(arylether nitrile) containing carboxylic acid groups is prepared by nucleophilic aromatic substitution polycondensation reaction, and free radical polymerization is performed with an olefin compound containing polyethylene glycol and an olefin compound containing phenylboronic acid structure, and then blended with polyvinylpyrrolidone to form a composite material with super mechanical properties and high thermal stability. Compared with traditional shape memory polymers, the composite material shows significant improvement in thermal properties, especially mechanical properties, and can maintain stable performance under harsh environmental conditions.

[0035] 3. The recyclable shape memory composite material with super mechanical properties provided by the present invention can be applied in various fields, especially in fields with high requirements for shape memory and mechanical properties, and has extremely high application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a stress-strain curve diagram of the shape memory composite material obtained in Example 1;

[0037] Figure 2 is a stress-strain curve diagram of the shape memory composite material obtained in Example 2;

[0038] Figure 3 is a stress-strain curve diagram of the shape memory composite material obtained in Example 3;

[0039] Figure 4 is a stress-strain curve diagram of the shape memory composite material obtained in Example 4;

[0040] Figure 5 is a stress-strain curve diagram of the shape memory composite material obtained in Example 5;

[0041] Figure 6 is a stress-strain curve diagram of the shape memory composite material obtained in Example 6;

[0042] Figure 7 is a stress-strain curve diagram of the shape memory composite material obtained in Example 7;

[0043] Figure 8 is a stress-strain curve diagram of the shape memory composite material obtained in Comparative Example 1;

[0044] Fig. 9 is a stress-strain curve diagram of the shape memory composite material obtained in Comparative Example 2;

[0045] Fig.10 is a differential scanning calorimetry diagram of the shape memory composite material obtained in Example 1;

[0046] Fig.11 This is a thermogravimetric analysis diagram of the shape memory composite material obtained in Example 1;

[0047] Fig.12 is a transmission electron microscope image of the shape memory composite material obtained in Example 1;

[0048] Fig.13 This is a macroscopic shape memory test diagram of the shape memory composite material obtained in Example 1;

[0049] Fig.14 This is a test diagram of the recyclability of the shape memory composite material obtained in Example 1. DETAILED DESCRIPTION

[0050] The embodiments of the present invention will be described in detail below in conjunction with examples. However, those skilled in the art will understand that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. The specific conditions not specified in the examples are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0051] The specific technical solution of the present invention is:

[0052] In a first aspect, the present invention provides a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties, wherein the composite material is represented by formula (I):

[0053] Formula (I) ;

[0054] Wherein, n is an integer between 80 and 100, x+y+z=1 and x>0, y>0, z>0; i is an integer between 270 and 3250;

[0055] Wherein, R1 is selected from formula (II) or formula (III);

[0056] The above formula (II) is , wherein m1 is an integer between 20 and 35, and R6 is selected from -H, substituted or unsubstituted C 1-18 A group consisting of an alkyl group;

[0057] The above formula (III) is , where m2 is an integer between 10 and 55;

[0058] Among them, R2 contains a phenylboronic acid structure.

[0059] The polymer of this scheme solves the problem of insufficient mechanical and thermal properties of existing shape memory polymers by introducing polyvinyl pyrrolidone and boron oxygen dynamic covalent bonds, as well as carboxylic acid groups into the molecular structure of polyarylethernitrile. The composite polymer material containing the above groups has high heat resistance, pressure resistance and chemical corrosion resistance, as well as excellent shape memory effect, can maintain stable performance under harsh environmental conditions, and is recyclable, meeting the requirements of green environmental protection and sustainable development.

[0060] Furthermore, in a preferred embodiment of the present invention, the above R6 is selected from -H, substituted or unsubstituted C 18 .

[0061] In a second aspect, the present invention provides a method for preparing a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties, comprising the following steps:

[0062] S1. Add bisphenol A, 2,6-dihalobenzonitrile, 2,2-diallylbisphenol A, phenolphthalein and a catalyst into a reaction container to obtain a mixed solution a, wherein the sum of the molar amounts of the three substances added, bisphenol A, 2,2-diallylbisphenol A and phenolphthalein, is equal to the molar amount of 2,6-dihalobenzonitrile;

[0063] Each halogen group of 2,6-dihalobenzonitrile can react with a hydroxyl group (from bisphenol A, 2,2-diallylbisphenol A or phenolphthalein) to form a phenol ether bond. Therefore, to ensure that each halogen group can find a corresponding hydroxyl group to participate in the reaction, the total molar number of hydroxyl groups needs to be equal to the total molar number of halogen groups. When the sum of the molar numbers of bisphenol A, 2,2-diallylbisphenol A, and phenolphthalein is equal to the molar number of 2,6-dihalobenzonitrile, the unreacted monomer can be minimized, and the generation of side reactions and by-products can also be reduced.

[0064] S2, adding the first solvent and the water-carrying agent to the mixed solution a, mixing well and then heating to boiling, reflux reaction until water is completely removed; continuing to heat the reaction system to 170-190° C., keeping the temperature for reaction for 1-2 hours, obtaining a reaction mixture containing polyarylethernitrile, precipitating the reaction mixture with an acidic solution, filtering, and drying to obtain a crude polyarylethernitrile containing a carboxylic acid group;

[0065] S3, dissolving the crude product obtained in step S2 in a first solvent, and then adding concentrated hydrochloric acid to acidify to obtain a polyarylether nitrile mixture containing carboxylic acid groups, adding anhydrous ethanol to the mixture until the precipitate no longer increases, filtering, boiling the filtrate with dilute hydrochloric acid, and then purifying and washing with pure water, and drying to obtain a polyarylether nitrile final product containing carboxylic acid groups;

[0066] S4, dissolving polyvinyl pyrrolidone and the polyarylether nitrile final product containing a carboxylic acid group in a second solvent, respectively, to obtain a polyvinyl pyrrolidone mixed solution and a polyarylether nitrile final product mixed solution containing a carboxylic acid group, respectively;

[0067] S5, adding monomer 1, monomer 2 and initiator to the final product mixed solution obtained in step S4, stirring and dissolving, and continuing to heat the reaction system to 60-80° C. and keep warm for 10-14 hours to obtain a shape memory polyarylene ether nitrile solution;

[0068] In step S5, the temperature is 60-80°C, and the initiator can effectively decompose to generate free radicals, thereby initiating the polymerization reaction of monomer 1 and monomer 2. Keeping the temperature for 10-14 hours can ensure that the reaction can proceed fully, so that the monomers can be fully polymerized to form high molecular weight polymers, which can ensure that the final material has excellent mechanical properties and shape memory properties.

[0069] The monomer 1 is selected from an olefin compound containing an R1 structure, and the monomer 2 is selected from an olefin compound containing a phenylboronic acid structure. The olefin compound is to react with the double bond in the allyl bisphenol A in the main chain. The R1 structure can be used as a soft segment in the polyarylethernitrile polymer, and the polyarylethernitrile main chain is used as a hard segment, which is a prerequisite for achieving shape memory performance. The R2 structure forms a dynamic boron-oxygen bond in the polyarylethernitrile polymer, giving the polymer a recyclable property while improving the shape memory performance.

[0070] S6, uniformly mixing the shape memory poly(arylene ether nitrile) solution prepared in step S5 with a polyvinyl pyrrolidone solution dissolved in a second solvent, and then evaporating the mixed solution to obtain a recyclable shape memory composite material having super mechanical properties;

[0071] Furthermore, in a preferred embodiment of the present invention, the above-mentioned monomer 1 is octadecyloxy polyethylene glycol methacrylate, polyethylene glycol methyl acrylate, polyethylene glycol ethyl methacrylate or allyl polyethylene glycol; and the above-mentioned monomer 2 is 3-vinylbenzeneboronic acid, 4-vinylbenzeneboronic acid or acrylamidophenylboronic acid.

[0072] Furthermore, in a preferred embodiment of the present invention, the above-mentioned monomer 1 is selected from allyl polyethylene glycol.

[0073] Furthermore, in a preferred embodiment of the present invention, the first solvent is N-methylpyrrolidone; the water-carrying agent is toluene; the catalyst is anhydrous potassium carbonate, sodium carbonate, potassium hydroxide or sodium hydroxide; the second solvent is N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

[0074] The first solvent choice is N-methylpyrrolidone (NMP), which is a polar solvent that has better solubility for poly(arylether nitrile) and has stable chemical properties at high temperatures, making it suitable for high-temperature polymerization reactions. Compared with other solvents such as dimethyl sulfoxide and N,N-dimethylformamide, NMP has a lower volatilization rate, which helps control the polymerization process and reduce environmental impact.

[0075] The second solvent is selected from dimethyl sulfoxide, N-methylpyrrolidone and N,N-dimethylformamide (DMF), because DMF has a better solubility for poly(arylene ether nitrile) than dimethyl sulfoxide and N-methylpyrrolidone, and can be more easily volatilized in the drying stage than NMP.

[0076] Toluene is a good non-polar solvent and is suitable as a water carrier, which can effectively help remove water. Toluene has a low boiling point (about 110°C), which is more helpful in removing water during the reaction.

[0077] Further preferably, in a preferred embodiment of the present invention, the catalyst is anhydrous potassium carbonate;

[0078] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the polyvinyl pyrrolidone and the poly(arylene ether nitrile) containing carboxylic acid groups in the above step S4 is 1-20:100.

[0079] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the polyvinyl pyrrolidone and the poly(arylene ether nitrile) containing carboxylic acid groups in the above step S4 is 5-15:100.

[0080] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the polyvinyl pyrrolidone and the poly(arylene ether nitrile) containing carboxylic acid groups in the above step S4 is 10:100.

[0081] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2 added in the above step S3 is 10:1-4:1-4.

[0082] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2 added in the above step S3 is 10:1-2:1-2.

[0083] Furthermore, in a preferred embodiment of the present invention, the mass ratio of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2 added in the above step S3 is 10:2:1.

[0084] Furthermore, in a preferred embodiment of the present invention, the molar ratio of the catalyst to 2,6-dihalobenzonitrile is 1:1-1.5; and the volume ratio of the water-carrying agent to the first solvent is 1:2-4.

[0085] Furthermore, in a preferred embodiment of the present invention, the mass of the initiator added in the above step S3 accounts for 0.2-2% of the total mass of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2.

[0086] Furthermore, in a preferred embodiment of the present invention, the mass of the initiator added in the above step S3 accounts for 0.4%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.6%, and 1.8% of the total mass of the three components of the polyarylethernitrile final product containing carboxylic acid groups, monomer 1 and monomer 2.

[0087] Further preferably, in a preferred embodiment of the present invention, the 2,6-dihalobenzonitrile is selected from 2,6-dichlorobenzonitrile and 2,6-difluorobenzonitrile.

[0088] In a third aspect, the present invention provides a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties for use in fields including aerospace, medical equipment, electronic equipment or smart textiles.

[0089] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0090] Example 1

[0091] A method for preparing a recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties comprises the following steps:

[0092] (1) 8.75 g of bisphenol A, 6 g of 2,2-diallyl bisphenol A, 11 g of 2,6-dichlorobenzonitrile, 2 g of phenolphthalein, and 10.8 g of anhydrous potassium carbonate were mixed to obtain a mixed solution a;

[0093] (2) Add 50 mL of the mixed solution a. N -Methyl pyrrolidone and 25 mL toluene are added to a 250 mL three-necked flask, stirred and mixed thoroughly, heated to 160 ° C and boiled, kept under reflux for 2 hours until the water is completely removed, then toluene is released, and the temperature is raised to 190 ° C at a rate of 10 ° C per hour and kept for 1 hour. When the viscosity of the reactant no longer changes, the reaction is terminated, and then poured into 1 mol / L hydrochloric acid until the reactant is completely precipitated, filtered and dried to obtain a crude polyarylethernitrile containing carboxylic acid groups;

[0094] (3) The crude polyarylethernitrile product is completely dissolved in N-methylpyrrolidone, and concentrated hydrochloric acid is added dropwise for acidification for 12 hours to obtain a polyarylethernitrile mixture containing carboxylic acid groups. Anhydrous ethanol is added to the mixture until the amount of precipitation no longer increases. After filtering, the filtrate is washed and purified with 1 mol / L hydrochloric acid and pure water respectively, and then the product is placed in a vacuum oven and completely dried to obtain a powdery polyarylethernitrile final product containing carboxylic acid groups.

[0095] (4) Weigh 1 g of polyvinyl pyrrolidone (molecular weight 360,000) and 10 g of powdered poly(arylethernitrile) containing carboxylic acid groups and dissolve them in 100 ml of N,N -dimethylformamide to obtain a mixed solution of polyvinyl pyrrolidone and a mixed solution containing a polyarylether nitrile product;

[0096] (5) Add 1 g of 4-vinylbenzeneboronic acid, 2 g of allyl polyethylene glycol and 0.26 g of initiator azobisisobutyronitrile to a mixed solution containing a poly(arylene ether nitrile) product, and stir to obtain a mixed solution; react the mixed solution at 70° C. for 12 h under a nitrogen atmosphere to obtain a shape memory poly(arylene ether nitrile) mixed solution.

[0097] (6) The shape memory poly(arylene ether nitrile) mixed solution and the poly(vinyl pyrrolidone) mixed solution were blended, the solution after the reaction was poured into a mold (40 mm×20 mm×5 mm), and dried at 60 °C for 24 h to obtain a shape memory composite material with ultra-high mechanical properties.

[0098] Example 2

[0099] (1) 7.25 g of bisphenol A, 6 g of 2,2-diallyl bisphenol A, 11 g of 2,6-dichlorobenzonitrile, 4 g of phenolphthalein, and 10.8 g of anhydrous potassium carbonate were mixed to obtain a mixed solution a;

[0100] (2) Add 60 mL of N-methylpyrrolidone and 20 mL of toluene to the mixed solution a and add them to a 250 mL three-necked flask. After being stirred and mixed thoroughly, the mixture is heated to 160° C. and boiled. The mixture is kept under reflux for 2 h until all water is removed. The toluene is then released and the mixture is heated to 180° C. at a rate of 10° C. per hour and kept warm for 2 h. The reaction is terminated when the viscosity of the reactant no longer changes. The mixture is then poured into 1 mol / L hydrochloric acid until the reactant is completely precipitated. The mixture is filtered and dried to obtain a crude poly(arylene ether nitrile) product containing a carboxylic acid group.

[0101] (3) The crude polyarylether nitrile product is completely dissolved in N-methylpyrrolidone, and concentrated hydrochloric acid is added dropwise for acidification for 12 hours to obtain a polyarylether nitrile mixture containing carboxylic acid groups. Anhydrous ethanol is added to the mixture until the amount of precipitation no longer increases. After filtering, the filtrate is washed and purified with 1 mol / L hydrochloric acid and pure water respectively, and then the product is placed in an oven and completely dried to obtain a powdery polyarylether nitrile final product containing carboxylic acid groups.

[0102] (4) Weighing 1.5 g of polyvinyl pyrrolidone (molecular weight: 360,000) and 10 g of a powdered poly(arylether nitrile) final product containing a carboxylic acid group, respectively, and dissolving them in 100 ml of N,N-dimethylformamide to obtain a polyvinyl pyrrolidone mixed solution and a mixed solution containing a poly(arylether nitrile) product, respectively;

[0103] (5) Add 1 g of 3-vinylbenzeneboronic acid, 2 g of allyl polyethylene glycol and 0.26 g of initiator azobisisobutyronitrile to a mixed solution containing a poly(arylene ether nitrile) product, and stir to obtain a mixed solution; react the mixed solution at 70° C. for 12 h under a nitrogen atmosphere to obtain a shape memory poly(arylene ether nitrile) mixed solution.

[0104] (6) The shape memory poly(arylene ether nitrile) mixed solution and the poly(vinyl pyrrolidone) mixed solution were blended, the solution after the reaction was poured into a mold (40 mm×20 mm×5 mm), and dried at 60°C for 24 h to obtain a shape memory composite material with ultra-high mechanical properties.

[0105] Example 3

[0106] (1) 8.75 g of bisphenol A, 4 g of 2,2-diallyl bisphenol A, 11 g of 2,6-dichlorobenzonitrile, 4 g of phenolphthalein, and 10.8 g of anhydrous potassium carbonate were mixed to obtain a mixed solution a;

[0107] (2) Add 60 mL of N-methylpyrrolidone and 25 mL of toluene to the mixed solution a and add them to a 250 mL three-necked flask. After stirring and mixing, heat the mixture to 160° C. and boil. Keep refluxing for 2 h until all water is removed. Then release toluene and heat the mixture to 180° C. at a rate of 10° C. per hour and keep the temperature for 2 h. When the viscosity of the reactant no longer changes, the reaction is terminated. Then, the mixture is poured into 1 mol / L hydrochloric acid until the reactant is completely precipitated. Filter and dry to obtain a crude poly(arylene ether nitrile) product containing a carboxylic acid group.

[0108] (3) The crude polyarylether nitrile product is completely dissolved in N-methylpyrrolidone, and concentrated hydrochloric acid is added dropwise for acidification for 12 hours to obtain a polyarylether nitrile mixture containing carboxylic acid groups. Anhydrous ethanol is added to the mixture until the amount of precipitation no longer increases. After filtering, the filtrate is washed and purified with 1 mol / L hydrochloric acid and pure water respectively, and then the product is placed in a vacuum oven and completely dried to obtain a powdery polyarylether nitrile containing carboxylic acid groups.

[0109] (4) Weighing 1.5 g of polyvinyl pyrrolidone (molecular weight: 360,000) and 10 g of a powdered poly(arylether nitrile) final product containing a carboxylic acid group, respectively, and dissolving them in 100 ml of N,N-dimethylformamide to obtain a polyvinyl pyrrolidone mixed solution and a mixed solution containing a poly(arylether nitrile) product, respectively;

[0110] (5) Add 1 g of 3-vinylbenzeneboronic acid, 2 g of allyl polyethylene glycol and 0.26 g of initiator azobisisobutyronitrile to a mixed solution containing a poly(arylene ether nitrile) product, and stir to obtain a mixed solution; react the mixed solution at 70° C. for 12 h under a nitrogen atmosphere to obtain a shape memory poly(arylene ether nitrile) mixed solution.

[0111] (6) The shape memory poly(arylene ether nitrile) mixed solution and the poly(vinyl pyrrolidone) mixed solution were blended, the solution after the reaction was poured into a mold (40 mm×20 mm×5 mm), and dried at 60°C for 24 h to obtain a shape memory composite material with ultra-high mechanical properties.

[0112] Example 4

[0113] Based on the method of Example 1, the amount of polyvinyl pyrrolidone and the final product of polyarylethernitrile containing carboxylic acid groups added in step (4) was changed, wherein 0.1 g of polyvinyl pyrrolidone and 10 g of the final product of polyarylethernitrile containing carboxylic acid groups were added, and the other steps were completely the same to obtain a shape memory composite material.

[0114] Example 5

[0115] Based on the method of Example 1, the amount of polyvinyl pyrrolidone and the final product of polyarylethernitrile containing carboxylic acid groups added in step (4) was changed, wherein 2 g of polyvinyl pyrrolidone and 10 g of the final product of polyarylethernitrile containing carboxylic acid groups were added, and the other steps were completely the same to obtain a shape memory composite material.

[0116] Example 6

[0117] In the method of Example 1, the type of the branched chain in step (5) was changed, 1 g of 4-vinylbenzene boronic acid, 2 g of octadecyloxy polyethylene glycol methacrylate and 0.26 g of initiator azobisisobutyronitrile were added to the mixed solution containing the poly(arylether nitrile) product, and stirred evenly to obtain a mixed solution; the mixed solution was reacted at 70° C. for 12 h under a nitrogen atmosphere to obtain a shape memory poly(arylether nitrile) mixed solution. The other steps were completely the same to obtain a shape memory composite material.

[0118] Example 7

[0119] In the method of Example 1, the molecular weight of polyvinyl pyrrolidone in step (4) was changed to 30,000, and the other steps were completely the same to obtain a shape memory composite material.

[0120] Comparative Example 1

[0121] Based on the method of Example 1, the amount of polyvinyl pyrrolidone and the final product of polyarylether nitrile containing carboxylic acid groups added in step (4) was changed, wherein polyvinyl pyrrolidone was not added, and 10 g of the final product of polyarylether nitrile containing carboxylic acid groups was added, and the other steps were completely the same, to obtain a shape memory composite material.

[0122] Comparative Example 2

[0123] In the method of Example 1, step (1) was changed to uniformly mix 10.2 g of bisphenol A, 6 g of 2,2-diallyl bisphenol A, 11 g of 2,6-dichlorobenzonitrile and 10.8 g of anhydrous potassium carbonate to obtain a mixed solution a; the other steps were completely the same to obtain a shape memory composite material.

[0124] In order to illustrate that the shape memory poly(arylene ether nitrile) composite material with ultra-high mechanical properties provided by the present application has good mechanical properties, thermal properties and shape memory effects, the following experiments are conducted:

[0125] Experimental Example 1: Mechanical Properties Test

[0126] The test method is as follows: the mechanical properties of the samples were tested by a universal testing machine at room temperature of 25°C and relative humidity of 25%. The dried samples were cut into dumbbell shapes, and the strain rate was set to 20 mm / min.

[0127] The mechanical properties of the composite materials obtained in Examples 1-7 and Comparative Examples 1-2 were tested respectively. The results are as follows: Figure 1-9 The stress-strain curve is shown in

[0128] The tensile strength of the composite material of Example 1 is 103 MPa, and the elongation at break is 19%; the tensile strength of the composite material of Example 2 is 95 MPa, and the elongation at break is 18%; the tensile strength of the composite material of Example 3 is 99 MPa, and the elongation at break is 16%; the tensile strength of the composite material of Example 4 is 77 MPa, and the elongation at break is 16%; the tensile strength of the composite material of Example 5 is 89 MPa, and the elongation at break is 15%; the tensile strength of the composite material of Example 6 is 97 MPa, and the elongation at break is 16%; the tensile strength of the composite material of Example 7 is 90 MPa, and the elongation at break is 19%;

[0129] The tensile strengths of Comparative Examples 1 and 2 are 61 MPa and 66 MPa, respectively. The mechanical properties of this embodiment are significantly higher than those of Comparative Examples 1 and 2.

[0130] Experimental Example 2: Thermal Performance Test

[0131] Test method: Mettler Toledo's STARe system was used for DSC analysis. The specific test method is as follows: First, the sample of Example 1 was dried using a temperature program of 70°C for 2 h, 90°C for 2 h, 110°C for 2 h, 130°C for 2 h, 150°C for 2 h, and 170°C for 2 h to ensure that the DMF solvent was completely evaporated. The sample was taken out and cooled to room temperature before testing. During the test, the sample was first heated to 40°C at a rate of 10ºC / min and kept at 40°C for 5 min; then heated to 260ºC at a rate of 10ºC / min and kept at 260 ºC for 5 min; then cooled to 40ºC at a rate of 10ºC / min and kept at 40ºC for 5 min; finally heated to 260ºC at a rate of 10ºC / min, and the nitrogen flow rate was always maintained at 50 mL / min during the test. Fig.10 , as shown in Figure 11. From the figure, it can be seen that the poly(arylethernitrile) composite material has excellent thermal properties, its glass transition temperature is 180℃, and the temperature is as high as 401℃ when the mass loss is 5%.

[0132] Experimental Example 3: Microstructure Test

[0133] Test method: The composite material prepared in Example 1 was tested on a JEM-2100F electron microscope with an operating voltage of 200 kV. Thin sections were sliced ​​using a Leica EM UC7 ultramicrotome with a thickness of about 100 nm and collected from the water surface onto a copper TEM grid. Then 5 µL of sodium phosphotungstate (NaTA) aqueous solution (1 wt%) was dropped onto the copper grid to selectively stain the carboxylic acid groups of the sample. The sliced ​​composite material was stained with sodium phosphotungstate (NaPT) and then subjected to TEM measurement. Fig.12 The TEM image in the figure clearly shows the bright spheres in the sliced ​​shape memory poly(arylethernitrile) composite, while the dark areas correspond to poly(arylethernitrile) containing carboxylic acid groups stained by sodium phosphotungstate. These bright spheres are hydrogen-bonded cross-linked nanoparticles of poly(arylethernitrile) and polyvinylpyrrolidone, which are hydrophobic and cannot be stained by sodium phosphotungstate.

[0134] The results show that:

[0135] Experimental Example 4: Shape Memory Test

[0136] Test method: The shape memory composite material prepared in Example 1 was made into a 20 mm × 2 mm × 0.2 mm rectangular parallelepiped strip, placed in an oven, heated at different temperatures, then bent into a "U" shape with external force, and then cooled to room temperature to obtain a temporary shape. The deformation angle was recorded as θ f The deformed spline is heated again to restore its original shape. At the same time, the angle (θ r ).like Fig.13 As shown, the shape memory composite material of Example 1 has an excellent shape memory recovery rate and can recover to its original shape within 75 seconds at a temperature of 110°C.

[0137] Experimental Example 5: Recycling Experiment Test

[0138] Test method: The recycling test uses a mixed solvent of DMF and ethanol. The recyclability test method is as follows: the shape memory composite material of Example 1 is completely dissolved in a mixed solvent of DMF and ethanol to obtain a polymer solution. Then, the polymer solution is poured into a rectangular polytetrafluoroethylene mold (40 mm×20 mm×5 mm), and then dried at 70°C until DMF is completely evaporated to obtain the recycled polymer.

[0139] like Fig.14 As shown, the poly(arylethernitrile) composite material is dissolved by a mixed solution of N,N-dimethylformamide and ethanol (v / v1=8:2) and then reshaped into a new shape after drying.

[0140] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A recyclable shape memory composite material based on poly(arylene ether nitrile) and having super mechanical properties, characterized in that: The composite material is represented by formula (I): Formula (I) ; Wherein, n is an integer between 80 and 100, x+y+z=1 and x>0, y>0, z>0; i is an integer between 270 and 3250; Wherein, R1 is selected from formula (III); The formula (III) is , where m2 is an integer between 10 and 55; Among them, the R2 formula contains a phenylboronic acid structure.

2. The method for preparing the shape memory composite material according to claim 1, characterized in that: The following steps are involved: S1. Add bisphenol A, 2,6-dihalobenzonitrile, 2,2-diallylbisphenol A, phenolphthalein and a catalyst into a reaction container, then add a first solvent and a water-carrying agent, mix well and heat to boiling, and reflux to react until all water is removed; continue to heat the reaction system to 170-190° C., keep the temperature for 1-2 hours to obtain a reaction mixture containing polyarylethernitrile, precipitate, filter and dry the reaction mixture to obtain a crude polyarylethernitrile containing a carboxylic acid group; S2, dissolving the crude product obtained in step S1 in a first solvent, and then adding concentrated hydrochloric acid to acidify to obtain a poly(arylene ether nitrile) mixture containing carboxylic acid groups, and sequentially precipitating, filtering, purifying, and drying the mixture to obtain a poly(arylene ether nitrile) final product containing carboxylic acid groups; S3, dissolving the final product obtained in step S2 in a second solvent, adding monomer 1, monomer 2 and an initiator, stirring and dissolving them, and continuing to heat the reaction system to 60-80° C. and keeping the temperature for 10-14 hours to obtain a shape memory polyarylethernitrile solution; S4, uniformly mixing the shape memory poly(arylene ether nitrile) solution prepared in step S3 with a polyvinyl pyrrolidone solution dissolved in a second solvent, and then evaporating the solvent to obtain a recyclable shape memory composite material having super mechanical properties; The monomer 1 is selected from olefin compounds containing R1 structure, and the monomer 2 is selected from olefin compounds containing phenylboronic acid structure.

3. The method for preparing the shape memory composite material according to claim 2, characterized in that: The monomer 1 is allyl polyethylene glycol; The monomer 2 is 3-vinylbenzeneboronic acid, 4-vinylbenzeneboronic acid or acrylamidobenzeneboronic acid.

4. The method for preparing the shape memory composite material according to claim 2, characterized in that: In the step S1, the sum of the molar quantities of bisphenol A, 2,2-diallylbisphenol A and phenolphthalein is equal to the molar quantity of 2,6-dihalobenzonitrile.

5. The method for preparing the shape memory composite material according to claim 2, characterized in that: The first solvent is N-methylpyrrolidone; the water-carrying agent is toluene; the catalyst is anhydrous potassium carbonate, sodium carbonate, potassium hydroxide or sodium hydroxide; the second solvent is N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

6. The method for preparing the shape memory composite material according to claim 2, characterized in that: The mass ratio of the polyvinyl pyrrolidone in step S4 to the poly(arylene ether nitrile) final product containing carboxylic acid groups obtained in step S2 is 1-20:

100.

7. The method for preparing the shape memory composite material according to claim 2, characterized in that: The mass ratio of the poly(arylene ether nitrile) final product containing carboxylic acid groups, monomer 1 and monomer 2 added in step S3 is 10:1-4:1-4.

8. The method for preparing the shape memory composite material according to claim 2, characterized in that: The molar ratio of the catalyst to 2,6-dihalobenzonitrile is 1:1-1.5; the volume ratio of the water-carrying agent to the first solvent is 1:2-4.

9. Application of a recyclable shape memory composite material with super mechanical properties as claimed in claim 1 or a recyclable shape memory composite material with super mechanical properties obtained by the preparation method described in any one of claims 2 to 8 in the fields of aerospace, medical equipment, electronic equipment or smart textiles.

Citation Information

Patent Citations

  • Cross-linking type polyarylene ether nitrile and preparation method thereof

    CN106046361A

  • Preparation method of high-performance carboxyl functionalized poly (arylene ether nitrile)

    CN109503826A

  • Blend, blend film and preparation method thereof, and applications of blend film in supercapacitors

    CN110776642A

  • Basalt fiber composite material with damage self-sensing capability and preparation method thereof

    CN116515274A

  • Repairable and recoverable shape memory thermosetting polymer based on polyarylene ether nitrile and preparation method thereof

    CN116903800A