Hyperbranched phosphonate polymer, preparation method thereof and polyester composition
By introducing the phosphaphenanthrene compound DOPO-HQ and hyperbranching agent into polyphosphonate, its molecular weight and flame retardancy are increased, which solves the problems of poor thermal stability and low mechanical properties of traditional polyphosphonate and achieves high performance. Preparation and flame retardant effect of polyester blend materials.
Patent Information
- Application Number
- CN202411014489.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
AI Technical Summary
Traditional polyphosphonates have poor thermal stability and are prone to bonding and clogging of feed lines. Linear polyphosphates have poor material mechanical properties. Existing hyperbranching agents are expensive or lead to excessive cross-linking, which affects Blending properties.
The phosphaphenanthrene compound DOPO-HQ is used with diaryl methylphosphonate and dihydric phenol to synthesize hyperbranched phosphonate. By adjusting the amount of hyperbranching agent, the molecular weight and glass transition temperature of the phosphonate are increased. , increase the phosphorus content, enhance flame retardancy and mechanical properties, and blend with polyester.
A hyperbranched phosphonate polymer with high glass transition temperature, low moisture absorption, excellent hydrolytic stability and light color is achieved, which is suitable for large-scale industrial production and has flame retardant properties after being added to polyester.
Smart Images

Figure BDA0004965313390000021 
Figure BDA0004965313390000091 
Figure BDA0004965313390000092
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardant chemical materials, and in particular to a hyperbranched phosphonate polymer used for a polymer flame retardant, a preparation method thereof and a polyester composition. Background Art
[0002] The synthetic raw materials of polyphenylphosphonate in traditional polyphosphonate are mainly phosphorus oxychloride, and the synthetic routes include interfacial polycondensation, solution method, melting method, etc. The molecular weight of the synthesized product is relatively low and the thermal stability is poor, which limits its application. In 2008, FRX Polymer Co., Ltd. used sodium phenolate as a catalyst instead of tetraphenylphosphine phenolate to improve the synthetic process conditions and obtained hyperbranched polymethylphosphonate, whose glass transition temperature is about 100°C and the maximum non-sintering temperature (MNST) is 120°C, but it is still relatively low compared with the processing temperature of PET. Before feeding to the extruder, PET needs to be dried at about 120°C to 150°C (higher than the Tg of polyphosphonate), so when the two polymers contact each other at the feed line of the extruder, they may stick together, thereby forming agglomerates and causing pressure fluctuations and / or blockage of the feed line. In addition, in a single screw extruder (SSE), the polyphosphonate polymer may enter the stage too early and cause lubrication on the barrel surface before the PET melts, which is not conducive to dispersion. In addition, linear polyphosphates are often synthesized with limited molecular weight, resulting in poor mechanical properties of the material.
[0003] Therefore, patent CN 1777632A mentions the introduction of a hyperbranching agent into polyphosphonate to increase its molecular weight, but the mentioned hyperbranching agent is relatively expensive. Patent CN 101802054A mentions the use of 1,1,1-tri(4-hydroxyphenyl)ethane as a hyperbranching agent for polyphosphonate, but this will result in the crosslinking degree of the prepared polyphosphate being too high, which is not conducive to blending, and will produce color, affecting the color of the blended polyester material itself. Summary of the invention
[0004] In order to solve the problems existing in the above-mentioned background technology, the present invention provides a hyperbranched phosphonate polymer and a preparation method thereof, wherein a phosphaphenanthrene compound DOPO-HQ is added to the synthesis of polyphosphate esters with phosphonate and dihydric phenol, and several hyperbranching agents with relatively low price that will not affect the color of the polyphosphonate are also added, and the molecular weight and Tg of the hyperbranched phosphonate polymer are regulated by controlling the amount of the hyperbranching agent, so that the hyperbranched phosphonate polymer can be fully melt-blended with polyester, and also has the characteristics of high phosphorus content, high melting point, Tg not less than 125°C, excellent hydrolysis stability, light color, easy preparation, etc. In addition, the present invention also adds the prepared polyphosphonate with a hyperbranched structure to polyester to prepare a polymer material with flame retardant properties.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The first aspect of the present invention provides a method for preparing a hyperbranched phosphonate polymer, comprising:
[0007] Add diaryl methylphosphonate, DOPO-HQ, dihydric phenol and / or diol, catalyst and hyperbranching agent into a reaction container, remove the generated phenol and excess diaryl methylphosphonate by heating and vacuuming, and form a hyperbranched phosphonate polymer.
[0008] Among the above-mentioned reaction raw materials, diaryl methylphosphonate is mainly selected from P-methyl-diphenylphosphonate (CAS No.: 7526-26-3); the Chinese name of DOPO-HQ is 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide, and its CAS No. is 99208-50-1. The dihydroxyphenyl contained in the structural formula can undergo an ester exchange reaction with diaryl methylphosphonate. Since DOPO-HQ contains P atoms and multiple aromatic ring structures, the selection of DOPO-HQ can increase the phosphorus content of the phosphonate polymer, enhance the flame retardancy of the phosphonate polymer and increase the glass transition temperature (Tg).
[0009] The chemical structure of DOPO-HQ is shown in formula (I):
[0010]
[0011] As a preferred technical solution, the ratio of the stoichiometric amount of the diaryl methylphosphonate to the stoichiometric amount of the DOPO-HQ, dihydric phenol and / or diol is 1.05 to 1.20.
[0012] As a preferred technical solution, the ratio of the stoichiometric amount of the DOPO-HQ input to the stoichiometric sum of the dihydric phenols and / or diols is 1:20 to 4:1, preferably 1:9 to 2:1.
[0013] As a preferred technical solution, the hyperbranching agent includes one or more of triphenyl phosphate, glycerol, pentaerythritol, trimethylolpropane, and phloroglucinol, and the stoichiometric amount of the hyperbranching agent added is 0.1-1% of the stoichiometric amount of diaryl methylphosphonate.
[0014] The hyperbranching agent selected in the present invention has the characteristics of 3-4 functional groups, light color and high reactivity. The molecular weight of the polyphosphonate is controlled by adjusting the addition amount of the hyperbranching agent, so as to achieve the purpose of enhancing the mechanical properties and glass transition temperature (Tg) of the polyphosphonate.
[0015] As a preferred technical solution, the dihydric phenol is selected from aromatic dihydric phenols including 6-20. Further, the dihydric phenol is one or more of catechol, resorcinol, hydroquinone, bisphenol S, and bisphenol A.
[0016] As a preferred technical solution, the diol is selected from 1-10 alkyl, 2-10 olefin or 5-10 cycloalkane diol. Further, the diol is one or more of ethylene glycol, propylene glycol, butylene glycol, isobutylene glycol, 1,5-pentanediol, neopentyl glycol, 2-methyl-1,4-butanediol, cyclopentane dimethanol and cyclohexanedimethanol.
[0017] As a preferred technical solution, the catalyst includes one or more of sodium phenolate, sodium 4-tert-butylphenolate, sodium p-methylphenolate, and tetraphenylphosphine phenolate. Further, the catalyst is sodium phenolate and / or tetraphenylphosphine phenolate, and the catalyst addition amount is 0.1-1wt% of the total raw material input, preferably 0.2-0.5wt%.
[0018] As a preferred technical solution, the specific steps of reacting the mixed system under heating and vacuum conditions are as follows: the first step is carried out at 100-200°C, the vacuum degree is 1k-100kPa, and the reaction time is 8-24h; the second step is carried out at 200-300°C, the vacuum degree is 5-1000Pa, and the reaction time is 6-12h.
[0019] Using the above technical solution:
[0020] (1) A phosphaphenanthrene compound DOPO-HQ is introduced into the reaction system. The structure of the DOPO-HQ compound contains a P atom and multiple aromatic ring structures. The dihydroxyphenyl group in the DOPO-HQ structure can undergo an ester exchange reaction with diaryl methylphosphonate, thereby increasing the phosphorus content of the obtained phosphonate polymer, so that the phosphonate polymer has the characteristics of high melting point, low moisture absorption rate, high thermal stability, high glass transition temperature (Tg), etc.
[0021] (2) A relatively inexpensive and light-colored hyperbranching agent is preferably used. Without affecting the color of the polymer, the molecular weight of the hyperbranched phosphonate polymer can be adjusted by adjusting the amount of the hyperbranching agent added, thereby achieving the purpose of improving the mechanical properties and glass transition temperature (Tg) of the polymer;
[0022] (3) The hyperbranched phosphonate polymer is prepared by a stepwise polycondensation process. The preparation method is simple, highly controllable, and easy to implement, suitable for large-scale industrial production, and realizes the simple preparation of hyperbranched phosphonate polymers with high glass transition temperature, transparency, hydrolysis stability, and controllable molecular weight.
[0023] The second aspect of the present invention provides a hyperbranched phosphonate polymer prepared by the above method, wherein the hyperbranched phosphonate polymer has a number average molecular weight of 30,000 to 100,000 and a glass transition temperature of ≥125°C.
[0024] The hyperbranched phosphonate polymer is heated in boiling water for 6 hours, and the hyperbranched phosphonate polymer forms less than 5% of degradation products.
[0025] The third aspect of the present invention provides a polyester composition, comprising the hyperbranched phosphonate polymer and other polyesters, wherein the phosphonate copolymer is added in an amount of 0.5 to 20 wt % in the polyester composition.
[0026] Specifically, the other polyesters are one or more of polybutylene terephthalate, polyethylene terephthalate, polypropylene terephthalate, polyethylene naphthalate, polybutylene 2,5-furandicarboxylate, polyethylene 2,5-furandicarboxylate, polypropylene 2,5-furandicarboxylate, and unsaturated polyesters.
[0027] In specific application, the polyester composition is composed of 0.5 to 20 wt% of a hyperbranched phosphonate polymer added to other polyesters, melt blended at 150 to 300° C. by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet with a thickness of 150 μm to 5000 μm; the cast thick sheet is then preheated to 100 to 180° C. and stretched longitudinally by 2 to 4 times, and then preheated again to 100 to 180° C. and stretched transversely by 2 to 4 times to obtain a polyester film or sheet with flame retardant properties.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) A phosphaphenanthrene compound DOPO-HQ is introduced into the reaction system. The structure of the DOPO-HQ compound contains a P atom and multiple aromatic ring structures. The dihydroxyphenyl group in the DOPO-HQ structure can undergo an ester exchange reaction with diaryl methylphosphonate, thereby increasing the phosphorus content of the obtained phosphonate polymer, so that the phosphonate polymer has the characteristics of high melting point, low moisture absorption rate, high thermal stability, high glass transition temperature (Tg), etc.
[0030] (2) A relatively inexpensive and light-colored hyperbranching agent is preferably used. Without affecting the color of the polymer, the molecular weight of the hyperbranched phosphonate polymer can be adjusted by adjusting the amount of the hyperbranching agent added, thereby achieving the purpose of improving the mechanical properties and glass transition temperature (Tg) of the polymer;
[0031] (3) The hyperbranched phosphonate polymer is prepared by a stepwise polycondensation process. The preparation method is simple, controllable, easy to implement, and suitable for large-scale industrial production. The hyperbranched phosphonate polymer with high glass transition temperature, transparency, hydrolysis stability, and controllable molecular weight is simply prepared;
[0032] (4) The prepared polyphosphonate with a hyperbranched structure can be added to polyester to prepare a polymer material with flame retardant properties. DETAILED DESCRIPTION
[0033] The technical solution of the present invention will be clearly and completely described below through specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention is further described below by way of examples. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commercially available products or products that can be prepared by known methods.
[0035] Example 1
[0036] 261 kg of diphenyl methylphosphonate, 30.8 kg of DOPO-HQ, 99 kg of hydroquinone, 0.4 kg of sodium phenol and 0.34 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 10 hours. Then, the temperature was continued to be heated to 270°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours, and then a light yellow hyperbranched phosphonate polymer was obtained.
[0037] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0038] The hyperbranched phosphonate polymer obtained in Example 1 was added to PBT polyester in an amount of 8 wt%, melt blended at 200°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet sample 1 with a thickness of 3200 μm.
[0039] Example 2
[0040] 265 kg of diphenyl methylphosphonate, 77 kg of DOPO-HQ, 44 kg of hydroquinone, 21.7 kg of ethylene glycol, 0.77 kg of sodium phenol and 1.05 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the mixture was heated to 260°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0041] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0042] The hyperbranched phosphonate polymer obtained in Example 2 was added to PET polyester in an amount of 5 wt%, melt blended at 220°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet sample 2 with a thickness of 3200 μm.
[0043] Example 3
[0044] 270 kg of diphenyl methylphosphonate, 107.8 kg of DOPO-HQ, 16.5 kg of hydroquinone, 52 kg of neopentyl glycol, 0.8 kg of sodium phenolate and 0.41 kg of phloroglucinol were added to the reactor, and the mixture was gradually heated from 100° C. to 200° C. At the same time, the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 12 hours. The mixture was then heated to 260° C., the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0045] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0046] The hyperbranched phosphonate polymer obtained in Example 3 was added to PEF polyester in an amount of 6 wt%, melt blended at 230°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet sample 3 with a thickness of 3200 μm.
[0047] Example 4
[0048] 275 kg of diphenyl methylphosphonate, 154 kg of DOPO-HQ, 22.83 kg of bisphenol A (228.286), 24.8 kg of ethylene glycol (62.068), 1.4 kg of sodium phenolate and 0.7 kg of phloroglucinol were added to a reactor, which was gradually heated from 100° C. to 200° C. At the same time, the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. The reaction was then continued to be heated to 280° C., and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0049] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0050] The hyperbranched phosphonate polymer obtained in Example 4 was added to PEN polyester in an amount of 5 wt%, melt blended at 240°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet sample 4 with a thickness of 3200 μm.
[0051] Example 5
[0052] 280 kg of diphenyl methylphosphonate, 184.8 kg of DOPO-HQ, 22.83 kg of bisphenol A, 31.2 kg of neopentyl glycol, 1.05 kg of tetraphenylphosphine phenolate and 0.62 kg of propylene glycol were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the reaction was continued to be heated to 240°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 9 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0053] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0054] The hyperbranched phosphonate polymer obtained in Example 5 is added to PTT polyester in an amount of 15 wt%, melt blended at 220°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet sample 5 with a thickness of 3200 μm.
[0055] Example 6
[0056] 285 kg of diphenyl methylphosphonate, 215.6 kg of DOPO-HQ, 25.03 kg of bisphenol S, 12.4 kg of ethylene glycol, 1.6 kg of tetraphenylphosphine phenolate and 0.85 kg of propylene glycol were added to the reactor, and the mixture was gradually heated from 100°C to 200°C. At the same time, the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. The mixture was then heated to 240°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 11 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0057] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0058] The hyperbranched phosphonate polymer obtained in Example 6 is added to the PBF polyester in an amount of 15 wt%, melt blended at 220°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet sample 6 with a thickness of 3200 μm.
[0059] Example 7
[0060] 290 kg of diphenyl methylphosphonate, 246.4 kg of DOPO-HQ, 25.03 kg of bisphenol S (250.27), 10.4 kg of neopentyl glycol, 2.0 kg of tetraphenylphosphine phenolate and 1.27 kg of pentaerythritol were added to a reactor, gradually heated from 100 ° C to 200 ° C, and at the same time, the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the mixture was heated to 240 ° C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 10 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0061] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0062] The hyperbranched phosphonate polymer obtained in Example 7 is added to the PTF polyester in an amount of 10 wt%, melt blended at 240°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet sample 7 with a thickness of 3200 μm.
[0063] Example 8
[0064] 297 kg of diphenyl methylphosphonate, 277.2 kg of DOPO-HQ, 22.4 kg of neopentyl glycol, 2.5 kg of tetraphenylphosphine phenolate and 1.63 kg of pentaerythritol were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the mixture was heated to 240°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 10 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0065] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0066] The hyperbranched phosphonate polymer obtained in Example 8 is added to the PBF polyester in an amount of 20 wt%, melt blended at 220°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet sample 8 with a thickness of 3200 μm.
[0067] Example 8
[0068] 297 kg of diphenyl methylphosphonate, 277.2 kg of DOPO-HQ, 22.4 kg of neopentyl glycol, 2.5 kg of tetraphenylphosphine phenolate and 1.63 kg of pentaerythritol were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the mixture was heated to 240°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 10 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0069] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0070] The hyperbranched phosphonate polymer obtained in Example 8 is added to the PBF polyester in an amount of 20 wt%, melt blended at 220°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid is cast onto a rotating cooling drum to obtain a cast thick sheet sample 8 with a thickness of 3200 μm.
[0071] Comparative Example 1
[0072] 261 kg of diphenyl methylphosphonate, 10.2 kg of DOPO-HQ, 106.37 kg of hydroquinone, 0.4 kg of sodium phenol and 0.34 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 10 hours. Then, the temperature was continued to be heated to 270°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours, and then a light yellow hyperbranched phosphonate polymer was obtained.
[0073] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0074] The hyperbranched phosphonate polymer obtained in Comparative Example 1 was added to PBT polyester in an amount of 8 wt%, melt blended at 200°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet comparison sample 1 with a thickness of 3200 μm.
[0075] Comparative Example 2
[0076] 290 kg of diphenyl methylphosphonate, 324 kg of DOPO-HQ, 18.37 kg of hydroquinone, 2.0 kg of tetraphenylphosphine phenolate and 1.27 kg of pentaerythritol were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 8 hours. Then, the mixture was heated to 240°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 10 hours to obtain a light yellow hyperbranched phosphonate polymer.
[0077] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0078] The hyperbranched phosphonate polymer obtained in Comparative Example 2 was added to the PTF polyester in an amount of 10 wt%, melt blended at 240°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet comparison sample 2 with a thickness of 3200 μm.
[0079] Comparative Example 3
[0080] 261 kg of diphenyl methylphosphonate, 109 kg of hydroquinone, 0.4 kg of sodium phenolate and 0.34 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 10 hours. Then, the temperature was continued to be heated to 270°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours, and then a light yellow hyperbranched phosphonate polymer was obtained.
[0081] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0082] The hyperbranched phosphonate polymer obtained in Comparative Example 1 was added to PBT polyester in an amount of 8 wt%, melt blended at 200°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet comparison sample 3 with a thickness of 3200 μm.
[0083] Comparative Example 4
[0084] 261 kg of diphenyl methylphosphonate, 30.8 kg of DOPO-HQ, 99 kg of hydroquinone, 0.4 kg of sodium phenol and 0.17 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 10 hours. Then, the temperature was continued to be heated to 270°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours, and then a light yellow hyperbranched phosphonate polymer was obtained.
[0085] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0086] The hyperbranched phosphonate polymer obtained in Example 1 was added to PBT polyester in an amount of 8 wt%, melt blended at 200°C by a mixer, then input into a single-screw or twin-screw extruder for melt extrusion, and the molten fluid was cast onto a rotating cooling drum to obtain a cast thick sheet comparison sample 4 with a thickness of 3200 μm.
[0087] Comparative Example 5
[0088] 261 kg of diphenyl methylphosphonate, 30.8 kg of DOPO-HQ, 99 kg of hydroquinone, 0.4 kg of sodium phenol and 4.1 kg of triphenyl phosphate were added to the reactor, gradually heated from 100°C to 200°C, and the primary vacuum pump was turned on to gradually reduce the air pressure from 100 kPa to 1000 Pa, and the reaction was carried out for 10 hours. Then, the temperature was continued to be heated to 290°C, and the secondary vacuum pump was turned on to gradually reduce the air pressure from 1000 Pa to 10 Pa, and the reaction was carried out for 8 hours, and then a light yellow hyperbranched phosphonate polymer was obtained.
[0089] The number average molecular weight, glass transition temperature, visible light transmittance of 1 mm sample film, and ratio of the mass of the prepared hyperbranched phosphonate copolymer after heating in boiling water for 6 hours to the original mass were tested. The test results are shown in Table 1.
[0090] The hyperbranched phosphonate polymer prepared in this comparative example has a too high melting point of 270° C., which is too different from the blending processing temperature of polyesters such as PET / PBT, so the blending sample cannot be prepared.
[0091] Table 1
[0092]
[0093] Since the hyperbranched phosphonate polymer prepared in Comparative Example 5 has a too high melting point of 270° C., which is too different from the blending processing temperature of polyesters such as PET / PBT, it is impossible to prepare a blended sample.
[0094] The flame retardancy test was performed on the cast thick sheet samples and cast thick sheet comparison samples prepared in Examples 1-8 and Comparative Examples 1-4. The test results are shown in Table 2.
[0095] In the following examples, the flame retardancy is determined according to the UL-94 flammability test to determine the fireproof standard of the sample. The sample is hot pressed into a strip of 125±5mm×13.0mm×4.0mm, and the sample is placed at 23°C and 50% humidity for testing. Each group of samples is tested 3 times, and the average value is taken. The fireproof grade of polyester is judged according to the three standards of V0, V1, and V2. The test results are shown in Table 2.
[0096] Table 2
[0097]
[0098]
[0099] From the test results in Table 1 and Table 2, it can be seen that the glass transition temperature of the phosphate copolymers prepared in Examples 1-8 is ≥125°C, and the number average molecular weight thereof is between 30,000 and 100,000. When the phosphonate copolymers are heated in boiling water for 6 hours, the phosphonate copolymers form less than 5% of degradation products. The phosphonate copolymers are made into a film with a thickness of not more than 1 mm, and the visible light transmittance is not less than 80%.
[0100] The polyester composition after adding the phosphonate polymer prepared in Examples 1-8 has a flame retardant property of UL-94V-0 level.
[0101] In the system of comparative example 1, the ratio of the input amount of DOPO-HQ to the stoichiometric sum of hydroquinone is about 1:29. The too low DOPO-HQ content in the system leads to a decrease in Tg, a large mass loss after 6 hours in boiling water, and a decrease in the flame retardant effect of the system. In the system of comparative example 2, the ratio of the input amount of DOPO-HQ to the stoichiometric sum of hydroquinone is about 5:1. The excessively high DOPO-HQ content in the system leads to a decrease in the molecular weight of the polyphosphonate, and the market price of DOPO-HQ is relatively high. Excessive input of DOPO-HQ will increase the production cost of the polyphosphonate, which is not conducive to large-scale production.
[0102] In Comparative Example 3, DOPO-HQ was not added to the reaction system, resulting in a further decrease in Tg and flame retardant effect, and the sample suffered a serious mass loss in boiling water.
[0103] The amount of the hyperbranching agent (triphenyl phosphate) added in the system of Comparative Example 4 is about 0.05%, and the too low content of the hyperbranching agent in the system results in a limited increase in the molecular weight of the polyphosphonate. The amount of the hyperbranching agent (triphenyl phosphate) added in the system of Comparative Example 5 is about 1.2%, and the too high content of the hyperbranching agent in the system results in serious crosslinking of the polyphosphonate, which cannot be melt-blended with polyesters such as PET / PBT, affecting processing and use.
[0104] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a hyperbranched phosphonate polymer, It is characterized in that include: Add diaryl methylphosphonate, DOPO-HQ, dihydric phenol and / or diol, catalyst and hyperbranching agent into a reaction container, remove the generated phenol and excess diaryl methylphosphonate by heating and vacuuming, and form a hyperbranched phosphonate polymer.
2. The method for preparing a hyperbranched phosphonate polymer according to claim 1, It is characterized in that The ratio of the stoichiometric amount of the diaryl methylphosphonate to the stoichiometric amount of the DOPO-HQ, dihydric phenol and / or diol is 1.05 to 1.
20.
3. The method for preparing the hyperbranched phosphonate polymer according to claim 1 or 2, It is characterized in that The ratio of the stoichiometric amount of the DOPO-HQ input to the stoichiometric sum of the dihydric phenol and / or dihydric alcohol is 1:20 to 4:
1.
4. The method for preparing a hyperbranched phosphonate polymer according to claim 1, It is characterized in that The hyperbranching agent includes one or more of triphenyl phosphate, glycerol, pentaerythritol, trimethylolpropane, and phloroglucinol. The stoichiometric amount of the hyperbranching agent added is 0.1-1% of the stoichiometric amount of diaryl methylphosphonate.
5. The method for preparing a hyperbranched phosphonate polymer according to claim 1, It is characterized in that The dihydric phenol is one or more of catechol, resorcinol, hydroquinone, bisphenol S and bisphenol A.
6. The method for preparing a hyperbranched phosphonate polymer according to claim 1, It is characterized in that The diol is one or more of ethylene glycol, propylene glycol, butylene glycol, isobutylene glycol, 1,5-pentanediol, neopentyl glycol, 2-methyl-1,4-butanediol, cyclopentane dimethanol, and cyclohexanedimethanol.
7. The method for preparing a hyperbranched phosphonate polymer according to claim 1, It is characterized in that The catalyst is sodium phenolate and / or tetraphenylphosphine phenolate, and the amount of the catalyst added is 0.1-1 wt % of the total raw materials input.
8. A hyperbranched phosphonate polymer, It is characterized in that It is prepared by the method described in any one of claims 1 to 7, the number average molecular weight of the hyperbranched phosphonate polymer is 30,000 to 100,000, and the glass transition temperature thereof is ≥125°C.
9. A polyester composition, It is characterized in that The invention comprises the hyperbranched phosphonate polymer as claimed in claim 8 and other polyesters, wherein the hyperbranched phosphonate copolymer is added in an amount of 0.5 to 20 wt % in the polyester composition.
10. The polyester composition according to claim 9, It is characterized in that The other polyesters are one or more of polybutylene terephthalate, polyethylene terephthalate, polypropylene terephthalate, polyethylene naphthalate, polybutylene 2,5-furandicarboxylate, polyethylene 2,5-furandicarboxylate, polypropylene 2,5-furandicarboxylate, and unsaturated polyesters.