Preparation method of degradable tableware hydrophobic coating
By reacting chitosan with acid solution and modifier, combined with zinc oxide and polylactic acid, a quaternary ammonium salt chitosan hydrophobic coating containing nano-zinc oxide was prepared, which solved the brittleness and gas permeability of the coating on degradable tableware. problem, achieving higher high temperature resistance and waterproof performance, while reducing production costs and improving antibacterial effects.
Patent Information
- Application Number
- CN202411142586.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-10-15
AI Technical Summary
Existing degradable hydrophobic coatings on degradable tableware have problems such as high brittleness, high gas permeability, poor antibacterial properties, and easy falling off.
Chitosan is mixed with acid solution, modifiers are added and the reaction proceeds to obtain quaternary ammonium salt chitosan, which is then combined with materials such as zinc oxide and polylactic acid to prepare quaternary ammonium salt containing nano-zinc oxide through ultrasonic dispersion and coating technology. Ammonium salt chitosan hydrophobic coating.
It improves the toughness and strength of the coating, enhances the barrier effect against water vapor, reduces production costs, and has good antibacterial properties and adhesion, meeting the conditions for use of disposable degradable tableware.
Smart Images

Figure BDA0005001305970000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating materials, and in particular to a method for preparing a degradable tableware hydrophobic coating. Background Art
[0002] With the popularity of fast food eating habits, disposable tableware has emerged. While it brings convenience and speed, it also has serious disadvantages such as ecological pollution and health and safety hazards. Therefore, new environmentally friendly and degradable tableware that is harmless to health has come into being. There are four main types of disposable degradable tableware that have been successfully developed: pulp mold tableware, plant fiber tableware, starch blended tableware, and degradable plastic tableware. Due to the particularity of the materials used in these four types of disposable degradable tableware, that is, they are not resistant to water, acid, alcohol, and oil, they cannot be used directly. In response to this type of problem, applying a hydrophobic coating on disposable degradable tableware is a routine operation in the prior art.
[0003] Polylactic acid is a completely biodegradable polymer material, which is eventually degraded into inorganic substances such as water and carbon dioxide by the enzyme action produced by microorganisms in the natural environment. It is gradually applied to various fields due to its advantages such as biodegradability, safety and hygiene, and low price. Some functional groups of polylactic acid are insoluble in water, which makes it have a certain hydrophobicity and can be used in the preparation of hydrophobic coatings. However, the strength of polylactic acid materials often cannot meet the requirements, with high brittleness, low heat deformation temperature, poor impact resistance, and high permeability of polylactic acid to organic gases, water vapor, CO2 and other gases, which cannot meet the use requirements of hydrophobic coating materials for degradable tableware. In view of the above problems, polylactic acid is usually mixed with other materials for processing, such as blending with reinforcing fillers, copolymerization modification, blending with other polymers, and composite modification to improve the comprehensive performance of polylactic acid, which can improve the barrier properties and mechanical properties of the material, but there are still problems such as poor modification effect, high modification cost, poor coating adhesion, and difficult to control degradation time. Therefore, it is urgent to invent a new type of degradable coating for degradable tableware. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a degradable tableware hydrophobic coating to solve the following technical problems:
[0005] The existing degradable hydrophobic coating applied on the surface of degradable tableware has the problems of high brittleness, variability, high gas permeability, poor antibacterial property and easy falling off.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a degradable tableware hydrophobic coating, the method for preparing the degradable tableware hydrophobic coating is prepared by the following method:
[0008] The chitosan and the acid solution are uniformly mixed, a modifier is added, and the mixture is reacted at 40-60° C. for 15-20 hours to obtain a quaternary ammonium salt chitosan solution, which is filtered, dialyzed, and dried to obtain a quaternary ammonium salt chitosan;
[0009] Dissolving zinc oxide in a quaternary ammonium salt chitosan aqueous solution, mixing evenly, ultrasonicating, centrifuging, taking the supernatant, and freeze-drying to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0010] The quaternary ammonium salt chitosan containing nano zinc oxide and a lubricant are added to a solvent, ultrasonically dispersed, polylactic acid is added, and the dispersion is continued for 1-2 hours, the substrate is coated, and the substrate is dried at room temperature to obtain the degradable tableware hydrophobic coating.
[0011] As a further embodiment of the present invention: the modifier is at least one of trimethyl ammonium chloride of triglyceride, octyl dodecyl dimethyl ammonium chloride, octyl tetradecyl dimethyl ammonium chloride, octyl hexadecyl dimethyl ammonium chloride, 3-chloro-2-hydroxypropyl trimethyl ammonium chloride, 2-hydroxypropyl dodecyl dimethyl ammonium chloride or 1,2-epoxypropyl dimethyl dodecyl ammonium chloride, and the mass ratio of the chitosan to the modifier is 1:1-3.
[0012] As a further solution of the present invention: the concentration of the quaternary ammonium salt chitosan aqueous solution is 1-2wt%.
[0013] As a further solution of the present invention: the acid solution is a 1-2% v / v acetic acid solution, and the addition ratio of the chitosan to the acid solution is 1 g: 30-50 mL.
[0014] As a further solution of the present invention: the mass ratio of the quaternary ammonium salt chitosan containing nano zinc oxide to the polylactic acid is 1:2-4.
[0015] As a further solution of the present invention: the solid-to-liquid ratio of the zinc oxide to the quaternary ammonium salt chitosan solution is 1:200-500, and the particle size of the zinc oxide is 3-8 μm.
[0016] As a further embodiment of the present invention: the solvent is one of dichloromethane, chloroform, acetone, dioxane, dimethylformamide, benzene or toluene, and the lubricant is glycerol.
[0017] As a further solution of the present invention: the thickness of the hydrophobic coating of the degradable tableware is 0.25-100.0 μm.
[0018] As a further embodiment of the present invention: the substrate is one of a pulp molded tableware substrate, a plant fiber type tableware substrate, a starch blended tableware substrate or a degradable plastic tableware substrate.
[0019] Beneficial effects of the present invention:
[0020] The degradable tableware coating obtained by the present invention is a completely biodegradable coating without any pollution. The present invention overcomes the shortcomings of the existing polylactic acid coating, such as low thermal deformation temperature, poor impact resistance and poor gas isolation, and successfully solves the problem of the existing products being difficult to isolate water vapor, thereby improving the toughness and strength of the product. At the same time, the raw materials used in the present invention are widely available, the preparation method is simple, the production cost is reduced, and the processing method of known equipment can be used for implementation, thereby reducing technical investment and facilitating promotion. Moreover, the product performance fully complies with the "Conditions for Use of Disposable Degradable Tableware".
[0021] In the hydrophobic coating of degradable tableware prepared by the present invention, quaternary ammonium salt chitosan containing nano zinc oxide is introduced into the polylactic acid coating substrate. Since polylactic acid contains a large number of hydrophobic groups C=O, the hydrophilic group -OH of the quaternary ammonium salt chitosan can react with it, thereby reducing the hydrophilicity of the quaternary ammonium salt chitosan and improving the barrier effect of the coating on water vapor, thereby preventing water vapor from penetrating the coating and damaging the degradable tableware substrate, thereby improving the high temperature resistance and waterproof performance of the degradable tableware.
[0022] It should be further explained that the use of quaternary ammonium chitosan has a better effect than the use of chitosan. Quaternary ammonium chitosan is easily soluble in water, and undergoes a grafting reaction with lactic acid through hydroxyl groups, which reduces hydrophilicity while retaining cationic quaternary ammonium groups. It can better combine with the tableware substrate through electrostatic action and improve the adhesion between the coating and the substrate. On the one hand, the grafting of quaternary ammonium chitosan with polylactic acid can reduce the amount of polylactic acid used. During the degradation process, the quaternary ammonium chitosan molecules will be decomposed first, achieving the effect of "breaking the whole into pieces" and increasing the degradation rate.
[0023] Nano zinc oxide is also introduced into the hydrophobic coating of the degradable tableware prepared by the present invention. The molecular chain of quaternary ammonium salt chitosan contains abundant amide and quaternary ammonium salt groups, has metal complexing ability, can load ZnO, avoid nano zinc oxide agglomeration, disperse nano ZnO particles into polylactic acid, occupy small holes in the polylactic acid structure, increase the cross-linking density of polylactic acid, increase the tensile performance of the polymer film, significantly increase the elongation at break and impact strength of the blend, and will not affect the biodegradable performance of polylactic acid, thereby improving the strength and toughness of the degradable tableware. At the same time, the quaternary ammonium chitosan can form a synergistic antibacterial effect with nano ZnO, thereby having a good antibacterial effect on Escherichia coli and Staphylococcus aureus. DETAILED DESCRIPTION
[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0027] Preparation of quaternary ammonium salt chitosan: weigh 1g chitosan and dissolve it in 35mL acetic acid (1.5% v / v) solution, dissolve 2g trimethylammonium chloride of triglyceride in 15mL deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium salt chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, obtain the purified quaternary ammonium salt chitosan by freeze drying;
[0028] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: 0.25 g zinc oxide was weighed and added to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), and stirred continuously for 24 hours, and then ultrasonicated in an ice bath for 10 hours, and then centrifuged at 4000 rpm for 10 minutes to remove the unstripped zinc oxide, and freeze-dried to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0029] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 0.8g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0030] Example 2
[0031] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0032] Preparation of quaternary ammonium salt chitosan: weigh 1g chitosan and dissolve it in 35mL acetic acid (1.5% v / v) solution, dissolve 2g trimethylammonium chloride of triglyceride in 15mL deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium salt chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, obtain the purified quaternary ammonium salt chitosan by freeze drying;
[0033] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: 0.25 g zinc oxide was weighed and added to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), and stirred continuously for 24 hours, and then ultrasonicated in an ice bath for 10 hours, and then centrifuged at 4000 rpm for 10 minutes to remove the unstripped zinc oxide, and freeze-dried to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0034] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 1g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0035] Example 3
[0036] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0037] Preparation of quaternary ammonium salt chitosan: weigh 1g chitosan and dissolve it in 35mL acetic acid (1.5% v / v) solution, dissolve 2g trimethylammonium chloride of triglyceride in 15mL deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium salt chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, obtain the purified quaternary ammonium salt chitosan by freeze drying;
[0038] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: 0.25 g zinc oxide was weighed and added to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), and stirred continuously for 24 hours, and then ultrasonicated in an ice bath for 10 hours, and then centrifuged at 4000 rpm for 10 minutes to remove the unstripped zinc oxide, and freeze-dried to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0039] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 1.2g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0040] Example 4
[0041] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0042] Preparation of quaternary ammonium salt chitosan: weigh 1g of chitosan and dissolve it in 35mL of acetic acid (1.5% v / v) solution, dissolve 1g of trimethylammonium chloride of triglyceride in 15mL of deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium salt chitosan by dialyzing it in deionized water through a dialysis bag for 3 days. Finally, obtain the purified quaternary ammonium salt chitosan by freeze drying;
[0043] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: 0.25 g zinc oxide was weighed and added to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), and stirred continuously for 24 hours, and then ultrasonicated in an ice bath for 10 hours, and then centrifuged at 4000 rpm for 10 minutes to remove the unstripped zinc oxide, and freeze-dried to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0044] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 0.8g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0045] Example 5
[0046] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0047] Preparation of quaternary ammonium chitosan: weigh 1g of chitosan and dissolve it in 35mL of acetic acid (1.5% v / v) solution, dissolve 3g of trimethylammonium chloride of triglyceride in 15mL of deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, lyophilize to obtain purified quaternary ammonium chitosan;
[0048] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: 0.25 g zinc oxide was weighed and added to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), and stirred continuously for 24 hours, and then ultrasonicated in an ice bath for 10 hours, and then centrifuged at 4000 rpm for 10 minutes to remove the unstripped zinc oxide, and freeze-dried to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0049] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 0.8g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0050] Example 6
[0051] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0052] Preparation of quaternary ammonium chitosan: weigh 1g of chitosan and dissolve it in 35mL of acetic acid (1.5% v / v) solution, dissolve 3g of trimethylammonium chloride of triglyceride in 15mL of deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, lyophilize to obtain purified quaternary ammonium chitosan;
[0053] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: weigh 0.2 g zinc oxide and add it to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), stir continuously for 24 hours, then ultrasonicate in an ice bath for 10 hours, then centrifuge at 4000 rpm for 10 minutes to remove the unpeeled zinc oxide, and freeze-dry to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0054] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 0.8g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0055] Example 7
[0056] A method for preparing a degradable tableware hydrophobic coating comprises the following steps:
[0057] Preparation of quaternary ammonium chitosan: weigh 1g of chitosan and dissolve it in 35mL of acetic acid (1.5% v / v) solution, dissolve 3g of trimethylammonium chloride of triglyceride in 15mL of deionized water, slowly drip the trimethylammonium chloride solution of triglyceride into the acetic acid solution containing chitosan, and stir at 55°C for 18h. Then, purify the quaternary ammonium chitosan by dialyzing it in deionized water for 3 days through a dialysis bag. Finally, lyophilize to obtain purified quaternary ammonium chitosan;
[0058] Preparation of quaternary ammonium salt chitosan containing nano zinc oxide: weigh 0.5 g zinc oxide and add it to 100 mL of quaternary ammonium salt chitosan aqueous solution (1 wt%), stir continuously for 24 hours, then ultrasonicate in an ice bath for 10 hours, then centrifuge at 4000 rpm for 10 minutes to remove the unpeeled zinc oxide, and freeze-dry to obtain quaternary ammonium salt chitosan containing nano zinc oxide;
[0059] Preparation of hydrophobic coating for degradable tableware: Weigh 0.4g of quaternary ammonium chitosan containing nano zinc oxide and 0.4g of glycerol, add them to 40g of chloroform solvent, ultrasonically disperse at 40°C and 25Hz for 1 hour, add 0.8g of polylactic acid, continue to disperse at 40°C and 10Hz for 2 hours, coat the polyethylene substrate, and dry at room temperature for 24 hours to obtain the hydrophobic coating for degradable tableware; the thickness of the polyethylene substrate is 1mm, and the thickness of the hydrophobic coating for degradable tableware is 50μm.
[0060] Comparative Example 1
[0061] Compared with Example 1, Comparative Example 1 omits the step of preparing quaternary ammonium salt chitosan containing nano zinc oxide, and directly mixes the purified quaternary ammonium salt chitosan with the lubricant and the solvent to prepare the coating. The remaining components and the preparation method are completely consistent with those in Example 1.
[0062] Comparative Example 2
[0063] Compared with Example 1, in Comparative Example 2, only 1 g of zinc oxide is added in the step of preparing quaternary ammonium salt chitosan containing nano zinc oxide, and the other components and preparation method are completely consistent with those of Example 1.
[0064] Comparative Example 3
[0065] Compared with Example 1, Comparative Example 3 omits the step of preparing quaternary ammonium salt chitosan, that is, 0.25 g zinc oxide is directly weighed and added into 100 mL chitosan aqueous solution (1 wt %), and the other components and preparation method are completely consistent with Example 1.
[0066] Comparative Example 4
[0067] Compared with Example 1, in Comparative Example 4, only in the step of preparing quaternary ammonium salt chitosan, 4 g of triglyceride trimethylammonium chloride was weighed and dissolved in 15 mL of deionized water, and the other components and preparation method were completely consistent with those of Example 1.
[0068] Comparative Example 5
[0069] Compared with Example 1, the preparation steps of quaternary ammonium chitosan and quaternary ammonium chitosan containing nano zinc oxide were omitted, 0.25g zinc oxide, 0.6g quaternary ammonium chitosan, and 0.4g glycerol were directly weighed and added to 40g chloroform solvent, and ultrasonically dispersed at 40°C and 25Hz for 1 hour, 0.8g polylactic acid was added, and the dispersion was continued at 40°C and 10Hz for 2 hours, and the polyethylene substrate was coated and dried at room temperature for 24 hours.
[0070] Performance Testing
[0071] The plate substrate coated with the degradable tableware hydrophobic coating obtained by the preparation method in Examples 1-7 and Comparative Examples 1-5 was cut to obtain samples with a size of 50 mm×50 mm, with a total of 4 samples in each group, and the test data was averaged.
[0072] Antimicrobial testing
[0073] The test was conducted according to the film-sticking method in Appendix C of the national standard GB / T 21510-2008 "Test Methods for Antibacterial Properties of Nano-inorganic Materials". The test bacteria were Staphylococcus aureus ATCC 25923 and Escherichia coli ATCC21320. The test results are shown in Table 1.
[0074] Table 1 Antibacterial rate test results of Examples 1-7 and Comparative Examples 1-5
[0075] Average inhibition rate of Escherichia coli / % Average inhibition rate of Staphylococcus aureus / % Example 1 99.9 99.9 Example 2 98.8 99.2 Example 3 98.4 97.4 Example 4 97.4 97.5 Example 5 98.5 98.2 Example 6 97.3 96.7 Example 7 97.5 97.9 Comparative Example 1 76.8 75.2 Comparative Example 2 79.5 79.6 Comparative Example 3 84.2 83.4 Comparative Example 4 85.2 84.5 Comparative Example 5 89.9 90.9
[0076] As shown in Table 1, the average antibacterial rate of the coating in Examples 1-7 is greater than 97%, and the average antibacterial rate of the coating in Comparative Examples 1 and 2 is the lowest, both lower than 80%, indicating that the quaternary ammonium chitosan containing nano ZnO and polylactic acid introduced in the present invention can form a synergistic antibacterial effect, avoiding the agglomeration of nano zinc oxide, thereby having a good antibacterial effect on Escherichia coli and Staphylococcus aureus. The average antibacterial rate of the coating in Comparative Example 5 is greater than the average antibacterial rate of the coating in Comparative Examples 1-4, indicating that the preparation method provided by the present invention can enable quaternary ammonium chitosan, nano ZnO and polylactic acid to form a better antibacterial effect.
[0077] Water vapor barrier performance test
[0078] The test was conducted according to ASTM-E96, using a W3 / 062 water vapor transmission rate meter (weight gain method) to measure water vapor transmission. The test temperature was (23±0.5)°C and the humidity was (50±1)% RH. The test results are shown in Table 2.
[0079] Oxygen barrier properties test
[0080] The oxygen permeability of the coating was measured using a Y110 oxygen permeability tester (pressure difference method test) at (23±0.1)°C and (50±2%) RH. The test results are shown in Table 2.
[0081] Table 2 Water vapor and oxygen barrier performance test results of Examples 1-7 and Comparative Examples 1-5
[0082] <![CDATA[Water vapor transmission rate / gm -2 d -1 > <![CDATA[Oxygen permeability (cm 3 m -2 d -1 > Example 1 8.2 7.3 Example 2 8.9 8.1 Example 3 8.4 7.9 Example 4 8.3 7.3 Example 5 9.1 8.6 Example 6 8.5 7.2 Example 7 8.4 7.6 Comparative Example 1 9.2 8.5 Comparative Example 2 9.3 8.0 Comparative Example 3 9.4 8.5 Comparative Example 4 9.4 8.6 Comparative Example 5 9.8 8.8
[0083] As shown in Table 2, the data of Examples 1-7 show that the degradable coating prepared by the present invention has good water vapor and oxygen barrier properties. The data of Example 2, Example 5 and Comparative Example 4 show that after increasing the content of quaternary ammonium salt chitosan grafted with polylactic acid containing nano zinc oxide, the water vapor permeability of the degradable tableware hydrophobic coating increases and the hydrophobic property decreases, indicating that adding quaternary ammonium salt chitosan beyond a certain range will reduce the hydrophobic property of the polylactic acid-based coating.
[0084] Contact angle: The static contact angle of the coating was measured using a DSA30 contact angle meter produced by Kruess, Germany. The test results are shown in Table 3.
[0085] Rolling angle: At room temperature, place the sample on a glass slide at an angle, drop a 10μL drop of water on it statically, and observe whether the water drop rolls on the sample. If it rolls, this angle is recorded as the rolling angle of the sample; if it does not roll, increase the number of glass slides until the water drop rolls on the sample. If the sample still does not roll at an angle of 90°, the rolling angle of the sample is recorded as 90°. The test results are shown in Table 3;
[0086] Adhesion performance: The adhesion of the coating was tested according to GB / T 9286-1998 "Scratch test for paint and varnish films". Six scratches were made on the coating sample in both the horizontal and vertical directions using a crosshatch knife. Then, 3M tape was used to completely adhere to the scratched area. The tape was quickly torn off at a 60° angle to the coating. The entire tearing time was controlled within 0.5-1s. The test results are shown in Table 3.
[0087] Table 3: Test results of contact angle, rolling angle and adhesion performance of Examples 1-7 and Comparative Examples 1-5
[0088]
[0089] It can be seen from Table 3 that the degradable tableware hydrophobic coating prepared in the present application has good mechanical properties and hydrophobicity. The introduction of quaternary ammonium chitosan containing nano zinc oxide into the polylactic acid-based coating improves the bonding strength between the coating and the degradable tableware substrate, thereby forming a surface coating with more stable bonding and higher strength. The addition amount of quaternary ammonium salt is within a certain range, which also improves the hydrophobicity of the coating surface.
[0090] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A method for preparing a degradable tableware hydrophobic coating, characterized in that: The preparation method of the degradable tableware hydrophobic coating is prepared by the following method: The chitosan and the acid solution are uniformly mixed, a modifier is added, and the mixture is reacted at 40-60° C. for 15-20 hours to obtain a quaternary ammonium salt chitosan solution, which is filtered, dialyzed, and dried to obtain a quaternary ammonium salt chitosan; Dissolving zinc oxide in a quaternary ammonium salt chitosan aqueous solution, mixing evenly, ultrasonicating, centrifuging, taking the supernatant, and freeze-drying to obtain quaternary ammonium salt chitosan containing nano zinc oxide; The quaternary ammonium salt chitosan containing nano zinc oxide and a lubricant are added to a solvent, ultrasonically dispersed, polylactic acid is added, and the dispersion is continued for 1-2 hours, the substrate is coated, and the substrate is dried at room temperature to obtain the degradable tableware hydrophobic coating.
2. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The modifier is at least one of triglyceride trimethylammonium chloride, octyldodecyldimethylammonium chloride, octyltetradecyldimethylammonium chloride, octylhexadecyldimethylammonium chloride, 3-chloro-2-hydroxypropyltrimethylammonium chloride, 2-hydroxypropyldodecyldimethylammonium chloride or 1,2-epoxypropyldimethyldodecylammonium chloride, and the mass ratio of chitosan to the modifier is 1:1-3.
3. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The concentration of the quaternary ammonium salt chitosan aqueous solution is 1-2 wt %.
4. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The acid solution is a 1-2% v / v acetic acid solution, and the addition ratio of chitosan to the acid solution is 1 g:30-50 mL.
5. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The mass ratio of the nano zinc oxide-containing quaternary ammonium salt chitosan to the polylactic acid is 1:2-4.
6. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The solid-liquid ratio of the zinc oxide to the quaternary ammonium salt chitosan solution is 1:200-500, and the particle size of the zinc oxide is 3-8 μm.
7. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The solvent is one of dichloromethane, chloroform, acetone, dioxane, dimethylformamide, benzene or toluene, and the lubricant is glycerol.
8. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The thickness of the degradable tableware hydrophobic coating is 0.25-100.0 μm.
9. The method for preparing a degradable tableware hydrophobic coating according to claim 1, characterized in that: The substrate is one of a pulp mold tableware substrate, a plant fiber tableware substrate, a starch blended tableware substrate, and a degradable plastic tableware substrate.
Citation Information
Cited By
Environment-friendly Non-PVC floor and preparation method thereof
CN119704835A