Preparation process of low-voltage anti-aging insulated cable

By using materials such as graphite phase carbon nitride powder and water-based antioxidants in low-voltage cables, the anti-aging performance and mechanical strength of the insulated cables are enhanced, the problems of insufficient anti-aging and mechanical strength in the existing technology are solved, and the More stable performance and longer service life.

CN118772474APending Publication Date: 2024-10-15KEYUE CABLE GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410979524.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing low-voltage cables have deficiencies in aging resistance and mechanical strength, making it difficult to meet increasingly stringent performance requirements. Especially during long-term use, they are easily affected by environmental factors, leading to performance degradation, and may even cause safety accidents.

Method used

Anti-aging coatings and water-based anti-aging agents are prepared using materials such as graphite phase carbon nitride powder and water-based antioxidant eutectic melt, combined with ingredients such as nano-silica, to enhance insulated cables through the synergistic effect of antioxidants and photoinitiators. Anti-aging properties and mechanical strength.

Benefits of technology

It significantly improves the anti-aging performance and mechanical strength of insulated cables, extends its service life, and shows a more stable anti-oxidation effect in aging tests, reducing performance degradation and safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772474A_ABST
    Figure CN118772474A_ABST
Patent Text Reader

Abstract

The invention provides a preparation process of a low-voltage anti-aging insulated cable, and belongs to the technical field of cables. The preparation process comprises the following steps: preparing the anti-aging coating; preparing a water-based anti-aging agent; and preparing the anti-aging insulated cable. The anti-aging coating is prepared, the graphite phase carbon nitride is added into the anti-aging coating, the graphite phase carbon nitride has good thermal stability and chemical stability and excellent chemical inertness, the binding force between polymer molecules can be greatly improved in the anti-aging coating, and the tensile strength of the coating is enhanced; the graphite-phase carbon nitride has a unique electronic structure, so that the graphite-phase carbon nitride has good light absorption capacity and has certain absorption and shielding effects on ultraviolet light, and the anti-aging performance and the mechanical strength of the insulated cable can be improved by coating the anti-aging coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cables, and in particular to a preparation process of a low-voltage anti-aging insulated cable. Background Art

[0002] Low-voltage cables are key components in power transmission and distribution systems and are widely used in commercial, residential and industrial fields. With the growing demand for electricity and higher expectations for grid reliability and life, the performance of low-voltage cables, especially their anti-aging performance, has become increasingly important. Although there are many types of low-voltage cables on the market, they still have certain limitations in terms of anti-aging and mechanical strength.

[0003] Anti-aging performance: During long-term operation, cables are affected by environmental factors such as temperature, humidity, ultraviolet radiation and chemical corrosion. Their insulation layer and sheath materials are prone to aging, resulting in performance degradation and even safety accidents.

[0004] Mechanical strength: The mechanical strength of cables is key to ensuring their proper operation and extended service life under high load conditions. However, many existing cables do not perform well in these aspects.

[0005] In view of the above problems, the low-voltage cables currently on the market are unable to meet the increasingly stringent performance requirements. Therefore, it is urgent to develop a new type of low-voltage anti-aging insulated cable, which should have excellent anti-aging performance and mechanical strength. Summary of the invention

[0006] In view of the deficiencies in the prior art, the present invention aims to provide a preparation process for a low-voltage anti-aging insulated cable.

[0007] A preparation process of a low-voltage anti-aging insulated cable comprises the following steps:

[0008] S1: Preparation of anti-aging coating

[0009] Graphite phase carbon nitride powder is prepared by melamine, the graphite phase carbon nitride powder is added to trimethylolpropane triacrylate to obtain a graphite phase carbon nitride diluent, the graphite phase carbon nitride diluent and a photoinitiator are added to a mixed polyurethane acrylate and stirred to obtain an anti-aging coating;

[0010] S2: Preparation of water-based antioxidant

[0011] The antioxidant 302 and the antioxidant 301 are mixed and completely melted to form an antioxidant eutectic, and then an emulsifier aqueous solution is added, stirred and cooled to obtain a water-based antioxidant;

[0012] S3: Preparation of anti-aging insulated cables

[0013] Low-density polyethylene and ethylene-vinyl acetate copolymer are mixed evenly, heated, and a cross-linking agent, a water-based anti-aging agent, a UV absorber, a plasticizer, and nano-silica are added. After mixing evenly, the mixture is extruded outside the cable core, cooled and formed to obtain an insulated cable. The anti-aging coating is coated on the insulated cable and cured to obtain an anti-aging insulated cable.

[0014] Furthermore, the preparation of the anti-aging coating in step S1 specifically comprises the following steps:

[0015] S1.1: 100-200 parts by weight of melamine is placed in a ceramic crucible with a lid, and then placed in a muffle furnace, and then heated to 550-560°C at a heating rate of 5-8°C / min and kept at this temperature for 3-4 hours, and then cooled naturally to obtain graphite phase carbon nitride powder;

[0016] S1.2: Add 2-3 parts by weight of graphite phase carbon nitride powder to 100-200 parts by weight of trimethylolpropane triacrylate, and grind for 2-3 hours using a basket grinder to obtain a graphite phase carbon nitride dilution solution;

[0017] S1.3: blending a difunctional aliphatic polyurethane acrylate, a tetrafunctional aliphatic polyurethane acrylate and a hexafunctional aliphatic polyurethane acrylate to obtain a mixed polyurethane acrylate;

[0018] S1.4: Add 30-40 parts by weight of graphite phase carbon nitride diluent and 5-8 parts by weight of photoinitiator to 100-200 parts by weight of mixed polyurethane acrylate, stir evenly, and obtain an anti-aging coating.

[0019] Furthermore, the preparation of the water-based anti-aging agent in step S2 specifically comprises the following steps:

[0020] S2.1: First, 40-50 parts by weight of antioxidant 302 is added into the reactor, and after it is completely melted, 60-70 parts by weight of antioxidant 301 is slowly added, and the two antioxidants are completely melted to form an antioxidant eutectic under heating conditions of 120-130° C. and constant temperature for 30-40 minutes;

[0021] S2.2: adding 10-20 parts by weight of an emulsifier to 30-50 parts by weight of deionized water, stirring and mixing to obtain an emulsifier aqueous solution;

[0022] S2.3: After cooling the antioxidant eutectic to 85-90°C, add the emulsifier aqueous solution and stir at 1000-1500 r / min for 20-30 min. Then, cool to room temperature under stirring at 100-200 r / min to obtain the water-based antioxidant.

[0023] Furthermore, step S3 of preparing the anti-aging insulated cable specifically comprises the following steps:

[0024] S3.1: 30-35 parts by weight of low-density polyethylene and 10-15 parts by weight of ethylene-vinyl acetate copolymer are mixed, stirred for 20-40 minutes, and heated to 70-80° C. to obtain a mixture;

[0025] S3.2: Add 0.5-1 parts by weight of a crosslinking agent, 1-2 parts by weight of an aqueous anti-aging agent, 1-2 parts by weight of an ultraviolet absorber, 1-2 parts by weight of a plasticizer, and 10-15 parts by weight of nano-silicon dioxide to the mixture, and stir for 10-20 minutes to obtain a mixture;

[0026] S3.3: Extruding the mixture outside the cable core, cooling and forming, obtaining a cable sheath, and making an insulated cable, applying the anti-aging coating evenly on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable.

[0027] Furthermore, in step S1.3, the difunctional aliphatic polyurethane acrylate, the tetrafunctional aliphatic polyurethane acrylate and the hexafunctional aliphatic polyurethane acrylate are blended in a ratio of 6-7:3:1.

[0028] Furthermore, in step S1.4, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone.

[0029] Furthermore, the emulsifier in step S2.2 is emulsifier A-105.

[0030] Furthermore, in step S3.2, the crosslinking agent is vinyltrimethoxysilane.

[0031] Furthermore, in step S3.2, the ultraviolet absorber is UV-531.

[0032] Furthermore, in step S3.2, the plasticizer is dibutyl phthalate.

[0033] Compared with the prior art, the present invention has at least the following beneficial effects:

[0034] 1. The present invention prepares an anti-aging coating, and adds graphite phase carbon nitride into the anti-aging coating. The graphite phase carbon nitride has good thermal stability and chemical stability, and has excellent chemical inertness. In the anti-aging coating, the bonding force between the graphite phase carbon nitride and the polymer molecules can be greatly improved, and the tensile strength of the coating can be enhanced. In addition, the graphite phase carbon nitride has a unique electronic structure, so it has good light absorption ability, and therefore has a certain absorption and shielding effect on ultraviolet light. Therefore, coating the anti-aging coating can improve the anti-aging performance and mechanical strength of the insulated cable.

[0035] 2. The present invention adopts a direct emulsification method to prepare a water-based antioxidant. The combination of antioxidants 302 and 301 can effectively inhibit the oxidation reaction of the insulated cable during use. By forming a eutectic, the antioxidant can be more evenly distributed in the cable material, providing a more stable and lasting antioxidant effect. Through the synergistic effect of the components, the water-based antioxidant has good compatibility with the material of the insulated cable, can better penetrate and combine, and thus more effectively exert the anti-aging effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings, which are incorporated herein and constitute a part of the specification, illustrate embodiments of the present disclosure and, together with the description, further serve to explain the principles of the present disclosure and to enable those skilled in the relevant art to make and use the present disclosure.

[0037] Figure 1 The present invention is a flow chart of a process for preparing a low-voltage anti-aging insulated cable used in an embodiment of the present invention. DETAILED DESCRIPTION

[0038] The following is a detailed description of a preparation process of a low-voltage anti-aging insulated cable provided by the present invention in conjunction with the accompanying drawings and specific embodiments. At the same time, it is explained here that in order to make the embodiments more detailed, the following embodiments are the best and preferred embodiments, and those skilled in the art may also adopt other alternatives to implement some known technologies; and the accompanying drawings are only for a more specific description of the embodiments, and are not intended to specifically limit the present invention.

[0039] Example 1

[0040] A preparation process for a low voltage anti-aging insulated cable, such as Figure 1 As shown, the following steps are included:

[0041] S1: Preparation of anti-aging coating

[0042] S1.1: 100 parts by weight of melamine is placed in a ceramic crucible with a lid, and then placed in a muffle furnace, and then heated to 550° C. at a heating rate of 5° C. / min and kept at this temperature for 3 h, and then cooled naturally to obtain graphite phase carbon nitride powder;

[0043] S1.2: Add 2 parts by weight of graphite phase carbon nitride powder to 100 parts by weight of trimethylolpropane triacrylate, and grind for 2 hours using a basket grinder to obtain a graphite phase carbon nitride dilution solution;

[0044] S1.3: blending a difunctional aliphatic polyurethane acrylate, a tetrafunctional aliphatic polyurethane acrylate and a hexafunctional aliphatic polyurethane acrylate in a ratio of 6:3:1 to obtain a mixed polyurethane acrylate;

[0045] S1.4: Add 30 parts by weight of graphite phase carbon nitride diluent and 5 parts by weight of 2-hydroxy-2-methyl-1-phenylacetone to 100 parts by weight of mixed polyurethane acrylate, stir evenly, and obtain an anti-aging coating;

[0046] S2: Preparation of water-based antioxidant

[0047] S2.1: First, 40 parts by weight of antioxidant 302 is added into the reactor, and after it is completely melted, 60 parts by weight of antioxidant 301 is slowly added, and the two antioxidants are completely melted to form an antioxidant eutectic under the condition of heating at 120°C for 30 minutes;

[0048] S2.2: Add 10 parts by weight of emulsifier A-105 to 30 parts by weight of deionized water, and stir to obtain an emulsifier aqueous solution;

[0049] S2.3: After cooling the antioxidant eutectic to 85°C, add the emulsifier aqueous solution, stir at 1000 r / min for 20 min, and then cool to room temperature under stirring at 100 r / min to obtain a water-based antioxidant;

[0050] S3: Preparation of anti-aging insulated cables

[0051] S3.1: 30 parts by weight of low-density polyethylene and 10 parts by weight of ethylene-vinyl acetate copolymer were mixed, stirred for 20 minutes, and heated to 70° C. to obtain a mixture;

[0052] S3.2: Add 0.5 parts by weight of vinyl trimethoxy silane, 1 part by weight of a water-based antioxidant, 1 part by weight of UV-531, 1 part by weight of dibutyl phthalate, and 10 parts by weight of nano-silicon dioxide to the mixture, and stir for 10 minutes to obtain a mixture;

[0053] S3.3: Extruding the mixture outside the cable core, cooling and forming, obtaining a cable sheath, and making an insulated cable, applying the anti-aging coating evenly on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable.

[0054] Example 2

[0055] A preparation process for a low voltage anti-aging insulated cable, such as Figure 1 As shown, the following steps are included:

[0056] S1: Preparation of anti-aging coating

[0057] S1.1: 200 parts by weight of melamine are placed in a ceramic crucible with a lid, and then placed in a muffle furnace, and then heated to 550° C. at a heating rate of 5° C. / min and kept at this temperature for 3 h, and then cooled naturally to obtain graphite phase carbon nitride powder;

[0058] S1.2: Add 3 parts by weight of graphite phase carbon nitride powder to 200 parts by weight of trimethylolpropane triacrylate, and grind for 2 hours using a basket grinder to obtain a graphite phase carbon nitride dilution solution;

[0059] S1.3: blending a difunctional aliphatic polyurethane acrylate, a tetrafunctional aliphatic polyurethane acrylate and a hexafunctional aliphatic polyurethane acrylate in a ratio of 7:3:1 to obtain a mixed polyurethane acrylate;

[0060] S1.4: Add 40 parts by weight of graphite phase carbon nitride diluent and 8 parts by weight of 2-hydroxy-2-methyl-1-phenylacetone to 200 parts by weight of mixed polyurethane acrylate, stir evenly, and obtain an anti-aging coating;

[0061] S2: Preparation of water-based antioxidant

[0062] S2.1: First, 50 parts by weight of antioxidant 302 is added into the reactor, and after it is completely melted, 70 parts by weight of antioxidant 301 is slowly added, and the two antioxidants are completely melted to form an antioxidant eutectic under the condition of heating at 120°C for 30 minutes;

[0063] S2.2: Add 20 parts by weight of emulsifier A-105 to 50 parts by weight of deionized water, and stir to obtain an emulsifier aqueous solution;

[0064] S2.3: After cooling the antioxidant eutectic to 85°C, add the emulsifier aqueous solution, stir at 1000 r / min for 20 min, and then cool to room temperature under stirring at 100 r / min to obtain a water-based antioxidant;

[0065] S3: Preparation of anti-aging insulated cables

[0066] S3.1: 35 parts by weight of low-density polyethylene and 15 parts by weight of ethylene-vinyl acetate copolymer were mixed, stirred for 20 minutes, and heated to 70° C. to obtain a mixture;

[0067] S3.2: Add 1 part by weight of vinyl trimethoxy silane, 2 parts by weight of water-based antioxidant, 2 parts by weight of UV-531, 2 parts by weight of dibutyl phthalate, and 15 parts by weight of nano-silicon dioxide to the mixture, and stir for 10 minutes to obtain a mixture;

[0068] S3.3: Extruding the mixture outside the cable core, cooling and forming, obtaining a cable sheath, and making an insulated cable, applying the anti-aging coating evenly on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable.

[0069] Example 3

[0070] A preparation process for a low voltage anti-aging insulated cable, such as Figure 1 As shown, the following steps are included:

[0071] S1: Preparation of anti-aging coating

[0072] S1.1: 100 parts by weight of melamine is placed in a ceramic crucible with a lid, and then placed in a muffle furnace, and then heated to 560° C. at a heating rate of 8° C. / min and kept at this temperature for 4 hours, and then cooled naturally to obtain graphite phase carbon nitride powder;

[0073] S1.2: Add 2 parts by weight of graphite phase carbon nitride powder to 100 parts by weight of trimethylolpropane triacrylate, and grind for 3 hours using a basket grinder to obtain a graphite phase carbon nitride dilution solution;

[0074] S1.3: blending a difunctional aliphatic polyurethane acrylate, a tetrafunctional aliphatic polyurethane acrylate and a hexafunctional aliphatic polyurethane acrylate in a ratio of 6:3:1 to obtain a mixed polyurethane acrylate;

[0075] S1.4: Add 30 parts by weight of graphite phase carbon nitride diluent and 5 parts by weight of 2-hydroxy-2-methyl-1-phenylacetone to 100 parts by weight of mixed polyurethane acrylate, stir evenly, and obtain an anti-aging coating;

[0076] S2: Preparation of water-based antioxidant

[0077] S2.1: First, 40 parts by weight of antioxidant 302 is added into the reactor, and after it is completely melted, 60 parts by weight of antioxidant 301 is slowly added, and the two antioxidants are completely melted to form an antioxidant eutectic under the condition of heating at 130°C for 40 minutes;

[0078] S2.2: Add 10 parts by weight of emulsifier A-105 to 30 parts by weight of deionized water, and stir to obtain an emulsifier aqueous solution;

[0079] S2.3: After cooling the antioxidant eutectic to 90°C, add the emulsifier aqueous solution, stir at 1500 r / min for 30 min, and then cool to room temperature under stirring at 200 r / min to obtain a water-based antioxidant;

[0080] S3: Preparation of anti-aging insulated cables

[0081] S3.1: 30 parts by weight of low-density polyethylene and 10 parts by weight of ethylene-vinyl acetate copolymer were mixed, stirred for 40 minutes, and heated to 80° C. to obtain a mixture;

[0082] S3.2: Add 0.5 parts by weight of vinyl trimethoxy silane, 1 part by weight of a water-based antioxidant, 1 part by weight of UV-531, 1 part by weight of dibutyl phthalate, and 10 parts by weight of nano-silicon dioxide to the mixture, and stir for 20 minutes to obtain a mixture;

[0083] S3.3: Extruding the mixture outside the cable core, cooling and forming, obtaining a cable sheath, and making an insulated cable, applying the anti-aging coating evenly on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable.

[0084] Comparative Example 1

[0085] Compared with Example 1, the difference of Comparative Example 1 is that Comparative Example 1 removes step S1 and step S3.3 of "evenly applying the anti-aging coating on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable", and the remaining steps remain unchanged to prepare the insulated cable, which is recorded as Comparative Example 1.

[0086] Comparative Example 2

[0087] Compared with Example 1, the difference of Comparative Example 2 is that Comparative Example 2 removes step S2, replaces the aqueous anti-aging agent in step S3.2 with an equal weight portion of antioxidant 1010, and prepares an anti-aging insulated cable without changing the other steps, which is recorded as Comparative Example 2.

[0088] The test methods for tensile strength, elongation at break and aging test performance are as follows:

[0089] Tensile Strength:

[0090] The tensile strength of the cable is measured in accordance with GB / T2951.11-2008 "General test methods for insulation and sheath materials of electrical and optical cables Part 11: General test methods - Thickness and dimensional measurement - Mechanical properties test".

[0091] Elongation at break:

[0092] The elongation at break of the cable is measured in accordance with GB / T2951.11-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 11: General test methods - Thickness and dimensional measurement - Mechanical properties test".

[0093] Aging test:

[0094] The cable aging test is carried out in accordance with GB / T2951.12-2008 "General test methods for insulation and sheath materials of electric and optical cables Part 12: General test methods-Heat aging test methods".

[0095] The tensile strength, elongation at break and aging tests were performed on Examples 1-3 and Comparative Example 1. The test results are shown in Table 1.

[0096] Table 1. Performance test results of Examples 1-3 and Comparative Example 1

[0097]

[0098] It can be seen from the data in Table 1 that the data of Comparative Example 1 are lower than those of the embodiment. Before aging, the tensile strength and elongation at break of Comparative Example 1 are lower than those of the embodiment, indicating that coating the anti-aging coating can improve the mechanical strength of the insulated cable; after aging, the change rate of Comparative Example 1 is higher than that of the embodiment, indicating that coating the anti-aging coating can improve the anti-aging performance of the insulated cable.

[0099] The aging data of Examples 1-3 are used, and an aging test is performed on Comparative Example 2. The measurement results are shown in Table 2.

[0100] Table 2. Aging test results of Examples 1-3 and Comparative Example 2

[0101] Tensile strength change rate (%) Change rate of elongation at break (%) Example 1 -0.7 -3.7 Example 2 -1.2 -4.1 Example 3 -0.9 -3.9 Comparative Example 2 -3.4 -7.3

[0102] It can be seen from the data in Table 2 that the change rates of Comparative Example 2 are higher than those of the embodiments, indicating that the aqueous antioxidant prepared by the direct emulsification method can provide a more stable and lasting antioxidant effect, and the aqueous antioxidant has good compatibility with the materials of the insulating cable, and can penetrate and combine better, thereby more effectively exerting the anti-aging effect, and effectively improving the anti-aging performance of the anti-aging insulating cable.

[0103] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A preparation process for a low-voltage anti-aging insulated cable, characterized in that: The steps include: S1: Preparation of anti-aging coating Graphite phase carbon nitride powder is prepared by melamine, the graphite phase carbon nitride powder is added to trimethylolpropane triacrylate to obtain a graphite phase carbon nitride diluent, the graphite phase carbon nitride diluent and a photoinitiator are added to a mixed polyurethane acrylate and stirred to obtain an anti-aging coating; S2: Preparation of water-based antioxidant The antioxidant 302 and the antioxidant 301 are mixed and completely melted to form an antioxidant eutectic, and then an emulsifier aqueous solution is added, stirred and cooled to obtain a water-based antioxidant; S3: Preparation of anti-aging insulated cables Low-density polyethylene and ethylene-vinyl acetate copolymer are mixed evenly, heated, and a cross-linking agent, a water-based anti-aging agent, a UV absorber, a plasticizer, and nano-silica are added. After mixing evenly, the mixture is extruded outside the cable core, cooled and formed to obtain an insulated cable. The anti-aging coating is coated on the insulated cable and cured to obtain an anti-aging insulated cable.

2. The preparation process of a low-voltage anti-aging insulated cable according to claim 1, characterized in that: Step S1: Preparation of anti-aging coating, specifically comprising the following steps: S1.1: 100-200 parts by weight of melamine is placed in a ceramic crucible with a lid, and then placed in a muffle furnace, and then heated to 550-560°C at a heating rate of 5-8°C / min and kept at this temperature for 3-4 hours, and then cooled naturally to obtain graphite phase carbon nitride powder; S1.2: Add 2-3 parts by weight of graphite phase carbon nitride powder to 100-200 parts by weight of trimethylolpropane triacrylate, and grind for 2-3 hours using a basket grinder to obtain a graphite phase carbon nitride dilution solution; S1.3: blending a difunctional aliphatic polyurethane acrylate, a tetrafunctional aliphatic polyurethane acrylate and a hexafunctional aliphatic polyurethane acrylate to obtain a mixed polyurethane acrylate; S1.4: Add 30-40 parts by weight of graphite phase carbon nitride diluent and 5-8 parts by weight of photoinitiator to 100-200 parts by weight of mixed polyurethane acrylate, stir evenly, and obtain an anti-aging coating.

3. The preparation process of a low-voltage anti-aging insulated cable according to claim 2, characterized in that: Step S2: Preparation of water-based anti-aging agent, specifically comprising the following steps: S2.1: First, 40-50 parts by weight of antioxidant 302 is added into the reactor, and after it is completely melted, 60-70 parts by weight of antioxidant 301 is slowly added, and the two antioxidants are completely melted to form an antioxidant eutectic under heating conditions of 120-130° C. and constant temperature for 30-40 minutes; S2.2: adding 10-20 parts by weight of an emulsifier to 30-50 parts by weight of deionized water, stirring and mixing to obtain an emulsifier aqueous solution; S2.3: After cooling the antioxidant eutectic to 85-90°C, add the emulsifier aqueous solution and stir at 1000-1500 r / min for 20-30 min. Then, cool to room temperature under stirring at 100-200 r / min to obtain the water-based antioxidant.

4. The preparation process of a low-voltage anti-aging insulated cable according to claim 3, characterized in that: Step S3: Preparation of anti-aging insulated cable, specifically comprising the following steps: S3.1: 30-35 parts by weight of low-density polyethylene and 10-15 parts by weight of ethylene-vinyl acetate copolymer are mixed, stirred for 20-40 minutes, and heated to 70-80° C. to obtain a mixture; S3.2: Add 0.5-1 parts by weight of a crosslinking agent, 1-2 parts by weight of an aqueous anti-aging agent, 1-2 parts by weight of an ultraviolet absorber, 1-2 parts by weight of a plasticizer, and 10-15 parts by weight of nano-silicon dioxide to the mixture, and stir for 10-20 minutes to obtain a mixture; S3.3: Extruding the mixture outside the cable core, cooling and forming, obtaining a cable sheath, and making an insulated cable, applying the anti-aging coating evenly on the insulated cable, placing it in a UV light box for curing reaction, and obtaining an anti-aging insulated cable.

5. The preparation process of a low-voltage anti-aging insulated cable according to claim 2, characterized in that: In step S1.3, the difunctional aliphatic polyurethane acrylate, the tetrafunctional aliphatic polyurethane acrylate and the hexafunctional aliphatic polyurethane acrylate are blended in a ratio of 6-7:3:

1.

6. The preparation process of a low-voltage anti-aging insulated cable according to claim 2, characterized in that: In step S1.4, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone.

7. The process for preparing a low-voltage anti-aging insulated cable according to claim 3, characterized in that: The emulsifier in step S2.2 is emulsifier A-105.

8. The process for preparing a low-voltage anti-aging insulated cable according to claim 4, characterized in that: In step S3.2, the crosslinking agent is vinyltrimethoxysilane.

9. The process for preparing a low-voltage anti-aging insulated cable according to claim 4, characterized in that: The ultraviolet absorber in step S3.2 is UV-531.

10. The process for preparing a low-voltage anti-aging insulated cable according to claim 4, characterized in that: In step S3.2, the plasticizer is dibutyl phthalate.