UiO-66 metal organic framework material as well as preparation method and application thereof
By using water as a precursor and high-temperature thermal activation in the synthesis of UiO-66, the problems of low efficiency and complex synthesis of traditional photocatalysts are solved, and the visible photocatalytic and efficient adsorption-photocatalytic removal performance of UiO-66 is achieved, simplifying the Process and reduce costs.
Patent Information
- Application Number
- CN202411254158.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-09
AI Technical Summary
Traditional photocatalysts are inefficient and have high synthesis costs. Conventional wastewater treatment processes cannot effectively remove low-concentration organic pollutants. Metal organic frame materials are complex in synthesis and low in yield, and the acidic conditions used are not conducive to large-scale reactions.
Water is used as the precursor additive to synthesize UiO-66 metal organic frame material through solvothermal reaction and high-temperature thermal activation methods, changing its electronic structure and pore structure, imparting its visible light excitation ability, and improving its adsorption-photocatalytic properties.
The visible photocatalytic capacity of UiO-66 is achieved, and its adsorption-photocatalytic removal performance of norfloxacin is improved, simplifies the synthesis process, reduces costs, and avoids the corrosion risk of acidic conditions.
Smart Images

Figure CN118930893A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal organic framework materials, and in particular to a UiO-66 metal organic framework material and a preparation method thereof. Background Art
[0002] The environmental pollution and health hazards of drugs and personal care products represented by antibiotics and non-steroidal anti-inflammatory drugs have become a hot topic of global concern. Although the concentration of these pollutants is extremely low (ng / L ~ μg / L), they are continuously discharged for a long time, have pseudo-persistence (resistance to light, chemical and biological degradation), and have more direct biological toxicity at low micro-concentrations (such as harm to the reproductive system, causing malignant tumors, leading to neurotoxicity, etc.), and are prone to cause bacterial resistance and resistance gene production and spread and other secondary environmental risks. These substances can penetrate conventional sewage treatment process (such as filtration, chlorination and ozone oxidation, etc.) into the water environment, so the conventional total quantification standards (total phosphorus, total nitrogen, COD, etc.) can no longer meet the high standards of water quality requirements.
[0003] Photocatalysis is a completely clean energy technology that can avoid the introduction of highly toxic or corrosive oxidants from Fenton or Fenton-like systems. Traditional photocatalytic reactions are inefficient due to the severe recombination of electrons and holes in semiconductor catalysts, and the development of emerging photocatalysts poses challenges to their synthesis costs. Combining adsorption technology with photocatalytic reactions can improve photocatalytic performance by shortening the distance between the pollutant and the catalyst interface. However, traditional semiconductor materials with photocatalytic properties show extremely low adsorption effects on most organic pollutants due to their low specific surface area and functional group sites.
[0004] Metal-organic frameworks (MOFs) are porous materials with high porosity and customized pore structures. They have broad application prospects in gas adsorption and adsorption of organic pollutants in water. MOFs are composed of metal clusters and organic ligands in alternating coordination. Therefore, they have the dual properties of organic and inorganic substances. In other words, MOFs can achieve the synthesis of multi-level pores through customized organic ligands to promote adsorption or catalytic mass transfer; aromatic organic ligands have a variety of functional groups to promote adsorption reactions; metal cluster sites can transfer electrons by synergistically absorbing light with organic ligands to form electron transfer from organic ligands to metal cluster sites or from metal clusters to organic ligands, thereby inhibiting the recombination of photogenerated carriers. However, the synthesis of MOFs is usually subject to strict reaction regulation and low yield.
[0005] Taking UiO-66 as an example, it usually needs to be synthesized in a reactor under high temperature and high pressure conditions; not only that, in order to obtain more perfect crystals, adding strong inorganic acids such as hydrofluoric acid and hydrochloric acid to the reaction precursor can slow down the protonation of the ligand, thereby slowing down the nucleation of the crystal; and adding monobasic strong organic acids, such as acetic acid or trifluoroacetic acid, can slow down the nucleation of the crystal by competitive coordination, and even adjust the multi-level pore structure. However, organic or inorganic strong acids usually have extremely strong corrosive ability and strong pungent odor, which brings difficulties to large-scale reaction design. The band gap of traditional UiO-66 is about 3.9 eV, and it can only be excited by ultraviolet light. This patent uses almost cost-free water as a precursor additive and cooperates with a high-temperature thermal activation process to simultaneously achieve the crystal synthesis, visible light excitation and adsorption performance improvement of UiO-66. Summary of the invention
[0006] The present invention provides a UiO-66 metal organic framework material and a preparation method and application thereof, and changes the precursor additive to enable UiO-66 to be excited by visible light.
[0007] In a first aspect, the present invention provides a method for preparing a UiO-66 metal organic framework material, comprising the following steps: S1. Dissolve the zirconium salt in a mixed solution of N,N-dimethylformamide and water, and fully dissolve it by ultrasonication; S2, after the solution is completely dissolved, add terephthalic acid and dissolve again by ultrasonication; S3, after dissolving, put it into an oven for heat preservation and reaction; S4, take out the product, wait for it to cool completely, and then wash it with N,N-dimethylformamide and then with methanol; S5. The washed product is vacuum dried to obtain the UiO-66 metal organic framework material.
[0008] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention introduces water into the precursor of UiO-66 through a simple solvothermal reaction to complete the synthesis of water-induced defective UiO-66; and induces the loss of ligands through vacuum heat treatment, thereby giving UiO-66 visible light catalytic ability, thereby simultaneously improving the pore structure and electronic structure of UiO-66, and promoting the adsorption-photocatalytic removal ability of norfloxacin.
[0009] Furthermore, the zirconium salt of S1 is ZrCl4, and the usage ratio of ZrCl4, N,N-dimethylformamide and water is 160 mg:40 mL:(0~100) equivalents, wherein 4 equivalents of water is equivalent to 0.05 mL of water.
[0010] Furthermore, the ultrasonic treatment time was 10 min.
[0011] Furthermore, in S3, the oven insulation temperature is 120° C. and the insulation time is 24 h.
[0012] Further, S4 was cleaned with N,N-dimethylformamide for 2 days, with the liquid being replaced every half day; and then cleaned with methanol for two days, with the liquid being replaced every half day.
[0013] Furthermore, the vacuum drying activation temperature in S5 is 80°C~200°C, and the drying time is 24h.
[0014] In the second aspect, the present invention provides a UiO-66 metal organic framework material obtained by the above method, named UiO-66-xeq-y, wherein x is the equivalent of added water, y is the vacuum activation temperature, and if there is no y mark, it means that it has not undergone high temperature activation.
[0015] In a third aspect, the present invention provides an application of a UiO-66 metal organic framework in treating norfloxacin in water. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The XRD patterns of the products obtained in Examples 5-9 and Comparative Example 2 of the present invention; Figure 2 The XRD patterns of the products obtained in Examples 1-4 and Comparative Example 1 of the present invention; Figure 3 The nitrogen adsorption-desorption spectra of the products obtained in Examples 1-4 and Comparative Example 1 of the present invention are shown; Figure 4 The pore size distribution diagram of the products obtained in Examples 1-4 of the present invention and Comparative Example 1; Figure 5 The electron paramagnetic resonance spectra of defective UiO-66 induced by activation with different equivalents of water and different temperatures provided by the present invention; Figure 6 The UV absorption spectra of the products obtained in Examples 1-3 and Comparative Example 1 of the present invention; Figure 7 The adsorption and photocatalytic degradation ability curves of Examples 1-3 of the present invention and Comparative Example 1 for 0.2 mg / L norfloxacin are shown. DETAILED DESCRIPTION
[0017] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto.
[0018] ZrCl4 metal salt, terephthalic acid organic ligand, N,N-dimethylformamide were used as solvent and glass bottle was used as reactor for the synthesis of MOF. Example 1
[0019] Dissolve 160 mg ZrCl4 in 40 mL DMF (N,N-2 methylformamide) and the corresponding amount of water (100 eq, eq means equivalent, 4eq=0.05mL), and ultrasonicate for 10 min. After complete dissolution, add 114.1 mg BDC (terephthalic acid), ultrasonicate for ten minutes, and then put it into a 120℃ oven for 24 h. After waiting for complete cooling, wash it with N,N-2 methylformamide for 2 days, changing the solvent every half a day; then wash it with methanol for two days, changing the solvent every half a day. Finally, vacuum dry it at 200℃ for 24 hours to obtain the sample named UiO-66-70eq-200. Example 2
[0020] The preparation process is the same as that in the example, except that the water equivalent is 50 eq, the vacuum drying temperature is 200° C., and the obtained sample is named UiO-66-50eq-200. Example 3
[0021] The preparation process is the same as that in the example, except that the water equivalent is 20 eq, the vacuum drying temperature is 200° C., and the obtained sample is named UiO-66-20eq-200.
[0022] Comparative Example 1 The preparation process is the same as that in the example, except that no water is added, the vacuum drying temperature is 200° C., and the obtained sample is named UiO-66-0eq-200. Example 4
[0023] The preparation process is the same as that in the example, except that the water equivalent is 100 eq, the vacuum drying temperature is 200° C., and the obtained sample is named UiO-66-100eq-200. Example 5
[0024] The preparation process is the same as that in the example, except that the water equivalent is 100 eq, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-100eq-80. Example 6
[0025] The preparation process is the same as that in the example, except that the water equivalent is 70 eq, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-70eq-80. Example 7
[0026] The preparation process is the same as that in the example, except that the water equivalent is 50 eq, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-50eq-80. Example 8
[0027] The preparation process is the same as that in the example, except that the water equivalent is 20 eq, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-20eq-80. Example 9
[0028] The preparation process is the same as that in the example, except that the water equivalent is 4 eq, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-4eq-80.
[0029] Comparative Example 2 The preparation process is the same as that in the example, except that no water is added, the vacuum drying temperature is 80° C., and the obtained sample is named UiO-66-0eq-80.
[0030] The samples obtained in Examples 1-9 and Comparative Examples 1-2 were subjected to X-ray diffraction testing. The results of the samples vacuum dried at an activation temperature of 200° C. are as follows: Figure 2 As shown, the results of the sample with vacuum drying activation temperature of 80°C are as follows Figure 1 As shown. The characteristic diffraction peaks of all samples can be well matched with the characteristic diffraction spectrum of UiO-66, which means the success of the synthesis. The incorporation of water promotes the nucleation of crystals within a certain range, and the main peak intensity of the X-ray diffraction spectrum increases (the peak intensity mentioned here is a point, and the other is to look at the broadening of the peak. It increases at 4eq, and the peak intensity decays later, but the decay is acceptable. After the water equivalent exceeds 70eq, whether it is 80℃ or 200℃, the peak appears to be broadened, which means that the crystallinity has been greatly damaged. It is believed that the sample no longer has the characteristics of UiO-66 at this time), but the crystal structure is damaged after the water equivalent exceeds 70 eq. After high-temperature activation, the relative diffraction intensity of all samples with water added to the precursors is significantly weakened, and even converted into an amorphous structure. This may be a defect caused by the falling of ligands under high temperature conditions.
[0031] Through experiments, it was found that adding water as a precursor additive promoted the decomposition of DMF and produced more formic acid ligands. Under high temperature (200°C), the formic acid ligands were removed, the electronic structure of MOF changed, the color became brighter, and the material had photocatalytic ability. At 80°C, the formic acid ligands could not be removed, the color remained unchanged, and the UiO-66 material obtained did not have photocatalytic ability. However, high temperature also destroyed the crystal structure of MOF, the specific surface area decreased, and the defects increased, so the adsorption performance decreased. In order to highlight the photocatalytic ability, samples under 200°C conditions (ie, Examples 1-4 and Comparative Example 1) were selected for nitrogen adsorption and desorption tests, and the results are as follows: Figure 3 , Figure 4 And as shown in Table 1. Figure 3 , Figure 4Table 1 reveals the pore structure of water-induced defective UiO after high-temperature activation. UiO-66-0eq-200 without water addition has almost no microporous structure. In contrast, with the increase of water addition, the specific surface area, micropore and mesopore volume of UiO-66 increased, but the change trend of specific surface area was different from the pore size distribution characteristics, which means that the addition of water regulates the growth of crystals and the formation of defects at the same time. When the water addition amount is 100 eq, the pore structure of UiO-66-100eq-200 is significantly weakened, which means that its crystal quality is greatly weakened.
[0032] Table 1 Data table of pore sizes of different samples sample <![CDATA[BET specific surface area (m 2 / g)]]> <![CDATA[Micropore volume (cm 3 / g)]]> <![CDATA[Mesoporous pore volume (cm 3 / g)]]> UiO-66-0eq-200 676 0.25 0.03 UiO-66-20eq-200 797 0.27 0.18 UiO-66-50eq-200 740 0.23 1.04 UiO-66-70eq-200 699 0.17 1.16 UiO-66-100eq-200 604 0.11 0.63 The present invention uses almost cost-free water as a precursor additive and cooperates with a high-temperature thermal activation process to simultaneously achieve the crystal synthesis, visible light excitation and adsorption performance improvement of UiO-66.
[0033] Electron paramagnetic resonance detection was performed on defective UiO-66 induced by activation with different equivalents of water and different temperatures. The results are as follows Figure 5 As shown; the products obtained in Examples 1-3 and Comparative Example 1 were subjected to ultraviolet light adsorption detection, and the results are as follows Figure 6 As shown. The electron paramagnetic resonance spectrum shows that the water-induced defective UiO-66 has an obvious free electron signal (g = 2.003, A < 10 G) after high-temperature activation, which is usually attributed to the formation of oxygen vacancies caused by missing ligands. The sample after high-temperature activation turned from the original white to yellow. Under high-temperature vacuum conditions, the crystal structure of MOFs may have changed, resulting in the adjustment of the electronic structure or band structure, which in turn affected the optical properties of the material. With the increase of water incorporation, the absorption of UiO-66 in the visible light range gradually increased. This means that the incorporation of water can cause a significant narrowing of the band gap by introducing missing joint defects in UiO-66. The change in color and the reduction in the band gap indicate the formation of missing joint defects. The removal of organic joints in UiO-66 leads to fewer bound oxygen states in the metal clusters, and the band gap is therefore reduced.
[0034] The samples obtained in Examples 1-3 and Comparative Example 1 were evaluated for the adsorption-photocatalytic performance of norfloxacin. The specific steps were as follows: the concentration of norfloxacin in the sewage was 200 μg / L, 50 mL of sewage was taken, 4 mg of the sample catalyst (the catalyst concentration after conversion was 0.08 g / L) was added, and a xenon lamp was used to simulate sunlight, and the light power density was 0.077 W / cm 2 , adsorption for 90 minutes, catalysis for 30 minutes. The adsorption was in the dark environment, and the catalysis was in the light. Liquid chromatography-mass spectrometry was used to quantitatively analyze the concentration of norfloxacin.
[0035] The results are as follows Figure 7 As shown in the figure, compared with UiO-66-0eq-200 without water regulation, other water-induced defective UiO-66 samples at an activation temperature of 200°C have achieved considerable improvement in adsorption and photocatalytic performance. Due to the most favorable pore structure and visible light absorption range of UiO-66-70eq-200, it finally showed excellent norfloxacin removal performance and completed the complete adsorption photocatalytic removal of 200 ppb norfloxacin.
[0036] Finally, it should be noted that the above are only preferred embodiments of the present invention. Of course, those skilled in the art can make changes and modifications to the present invention. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the scope of protection of the present invention.
Claims
1. A method for preparing a UiO-66 metal organic framework material, characterized in that: The steps include: S1. Dissolve the zirconium salt in a mixed solution of N,N-dimethylformamide and water, and fully dissolve it by ultrasonication; S2, after the solution is completely dissolved, add terephthalic acid and dissolve again by ultrasonication; S3, after dissolving, put it into an oven for heat preservation and reaction; S4, take out the product, wait for it to cool completely, and then wash it with N,N-dimethylformamide and then with methanol; S5. The washed product is vacuum dried to obtain the UiO-66 metal organic framework material.
2. The method for preparing the UiO-66 metal organic framework material according to claim 1, characterized in that: The zirconium salt of S1 is ZrCl4, and the dosage ratio of ZrCl4, N,N-dimethylformamide and water is 160 mg:40 mL:(0~100) equivalents, wherein 4 equivalents of water is equivalent to 0.05 mL of water.
3. The method for preparing the UiO-66 metal organic framework material according to claim 1, characterized in that: The ultrasonic treatment time was 10 min.
4. The method for preparing the UiO-66 metal organic framework material according to claim 1, characterized in that: The oven insulation temperature in S3 is 120°C and the insulation time is 24h.
5. The method for preparing the UiO-66 metal organic framework material according to claim 1, characterized in that: S4 was cleaned with N,N-dimethylformamide for 2 days, changing the liquid every half a day; and then cleaned with methanol for two days, changing the liquid every half a day.
6. The method for preparing the UiO-66 metal organic framework material according to claim 1, characterized in that: The vacuum drying activation temperature in S5 is 80℃~200℃, and the drying time is 24h.
7. The UiO-66 metal organic framework material prepared by the preparation method of the UiO-66 metal organic framework material according to any one of claims 1 to 6.
8. Use of the UiO-66 metal organic framework material according to claim 7 in treating norfloxacin in water.
Citation Information
Patent Citations
Defect type UiO-66 photocatalytic material, and preparation method and application thereof
CN113559936A
Micro-mesoporous UiO-metal organic framework material for reverse shape-selective adsorption separation of isoparaffin
CN114307975A
Defective zirconium-based metal organic framework adsorbent and preparation method thereof
CN115869924A
Modified UiO-66 material as well as preparation method and application thereof
CN117258766A
Method for manufacturing UiO-66 with specific micropore volume
CN117377678A
Cited By
Method for detecting levodopa
CN120870283A