Double-layer collagen sponge as well as preparation method and application thereof
By using freeze-drying and vacuum dry-heat cross-linking technologies in the preparation of collagen sponges, a double-layer collagen sponge is formed, which solves the problems of complex process, high cost and poor quality of collagen sponges in the existing technology, and achieves Efficient and safe preparation of collagen sponges for a variety of medical applications.
Patent Information
- Application Number
- CN202310367205.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-15
AI Technical Summary
The existing collagen sponge preparation process has problems such as the risk of reagent residue, long production cycle, high cost and poor product quality. In particular, the material is easily denatured in a high-temperature oxidizing environment, resulting in poor product quality.
A double-layer collagen sponge is prepared by configuring the collagen into a solution and then freeze-drying, and then uses a superconducting thermal plate in a vacuum drying oven for dry heat cross-linking and radiation cross-linking to form a loose layer and a dense layer. The double-layer structure improves the mechanical properties and biocompatibility of the product.
It achieves good intra-batch and inter-batch stability, high yield, improved mechanical properties, mechanical properties and anti-degradation properties, while reducing production costs. The product has good biocompatibility and low immunogenicity, and is suitable for large batches. Production.
Smart Images

Figure CN118772481A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical surgery, and in particular relates to a collagen sponge prepared based on an improved dry heat cross-linking technology and an application thereof. Background Art
[0002] Extensive bleeding and oozing are common problems encountered during surgical and traumatic operations, especially in multi-vascular solid organs, such as bleeding from liver trauma. Trauma is often accompanied by coagulation dysfunction caused by massive blood loss. Therefore, timely and effective hemostasis is the key to reducing the risk of postoperative death and improving postoperative recovery.
[0003] At present, domestic and foreign research can generally divide hemostatic materials into three categories according to the material: inorganic hemostatic materials, synthetic hemostatic materials and bio-derived hemostatic materials. Inorganic hemostatic materials mainly include zeolite, kaolin, montmorillonite, etc., which mainly absorb a large amount of water in the blood through molecular sieve action, thereby accelerating the formation of blood clots. The representative of inorganic hemostatic materials is the zeolite hemostatic material QuikClot, which is mainly used to stop bleeding in life-threatening injuries, but its non-degradable and exothermic characteristics limit its clinical application. Synthetic hemostatic materials are mostly medical adhesives, mainly including cyanoacrylate tissue glue, polyethylene glycol gel, etc. This type of hemostatic material does not have any endogenous hemostatic function, and mainly achieves the purpose of rapid bonding and sealing of traumatic tissues through cross-linking reactions or rapid polymerization at the wound site. Although this material can provide temporary protection and hemostasis for the wound, its shortcomings are obvious: 1. It has no effect on promoting wound healing; 2. Incomplete debridement can easily cause purulent infection of the wound, which brings new pain to the patient and prolongs the condition. Bio-derived hemostatic materials can be divided into two categories: protein hemostatic materials and polysaccharide hemostatic materials. The main sources of protein hemostatic materials include collagen, gelatin, fibrinogen, etc. The main sources of polysaccharide hemostatic materials include cellulose, starch, alginate, chitosan and other polysaccharides. Bio-derived hemostatic materials are increasingly valued by experts and scholars due to their non-toxicity, good biocompatibility, biodegradability and procoagulant activity, and their application prospects are very broad.
[0004] Animal-derived collagen has been widely used in the field of medical devices, and has been studied in depth in areas such as hemostasis and tissue repair, solving many clinical problems and benefiting many patients. In recent years, more and more scientific researchers have also been conducting in-depth research on recombinant bionic collagen obtained by genetic engineering. Compared with animal-derived collagen, this type of collagen has advantages such as no virus risks, good water solubility, and lower immunogenicity, so it is theoretically safer to use in the clinical field.
[0005] In addition, the process from the beginning of coagulation to the formation of thrombin is composed of two systems: endogenous and exogenous. Calcium ions are called coagulation factor IV in the coagulation mechanism. They are cofactors of multiple factors and can gradually convert prothrombin into thrombin together with other coagulation factors, participating in multiple links of the endogenous and exogenous coagulation pathways.
[0006] The recombinant collagen sponge material involved in invention patent ZL 202010052422.9 is cross-linked with chemical reagents, which poses risks such as reagent residues, and the reagent residues need to be removed during the process. The entire process is cumbersome, the production cycle is long, and the cost is high. Therefore, it is urgent to study a safer, more effective and cheaper collagen sponge.
[0007] Dry heat cross-linking technology has been widely used in medical materials, such as degradable hemostatic materials prepared by dry heat cross-linking of starch-chitosan, porous composite materials prepared by dry heat cross-linking of elastin-silk fibers, and three-dimensional porous scaffolds prepared by dry heat cross-linking of collagen-chitosan, etc. However, they all use ordinary ovens, and the materials are easily oxidized and denatured in an aerobic and high-temperature environment, resulting in poor product quality, which does not meet our expectations. Summary of the invention
[0008] In order to solve the above problems, the purpose of the present invention is to provide a double-layer collagen sponge and a preparation method and application thereof. The biofilm prepared by this method has a loose layer and a dense layer, and has good intra-batch and inter-batch stability, a high yield rate, and good mechanical properties, mechanical properties, swelling properties, anti-degradation properties, and biocompatibility.
[0009] In order to achieve the above object, the present invention provides a method for preparing a double-layer collagen sponge, which comprises the following steps:
[0010] (1) preparing collagen into a collagen solution;
[0011] (2) freeze-drying the collagen solution to obtain a collagen sponge;
[0012] (3) subjecting the collagen sponge to dry heat crosslinking and radiation crosslinking under vacuum conditions to obtain the double-layer collagen sponge;
[0013] Wherein, in step (3), dry heat crosslinking is carried out on a super heat conducting plate in a vacuum drying oven.
[0014] According to a specific embodiment of the present invention, preferably, in step (1), the collagen is recombinant collagen.
[0015] According to a specific embodiment of the present invention, preferably, the recombinant collagen is the recombinant human collagen disclosed in CN106554410A, and the recombinant human collagen comprises one or more of the following family members:
[0016] 1) A protein having an amino acid residue sequence of SEQ ID No: 1 in the sequence list;
[0017] 2) a protein derived from SEQ ID No: 1 that has an amino acid residue sequence homology of more than 90% with SEQ ID No: 1 and has the same activity as SEQ ID No: 1;
[0018] 3) a protein derived from SEQ ID No: 1 having the same activity as SEQ ID No: 1 obtained by adding or deleting up to 15 amino acid residues at the N-terminus of the amino acid residue sequence of SEQ ID No: 1;
[0019] 4) a protein derived from SEQ ID No: 1 having the same activity as SEQ ID No: 1 obtained by adding or deleting up to 15 amino acid residues at the C-terminus of the amino acid residue sequence of SEQ ID No: 1;
[0020] 5) A protein derived from SEQ ID No: 1, wherein one or more amino acid residues are substituted, deleted or added to the amino acid residue sequence of SEQ ID No: 1 and the protein has the same activity as SEQ ID No: 1.
[0021] According to a specific embodiment of the present invention, preferably, the concentration of collagen in the collagen solution is 0.5-15%, more preferably 1-10%, and further preferably 1-7%.
[0022] According to a specific embodiment of the present invention, preferably, in step (1), the composition of the collagen solution also includes an inorganic calcium salt, such as anhydrous calcium chloride (CaCl 2 ), which can promote the body's own endogenous hemostasis process.
[0023] According to a specific embodiment of the present invention, preferably, the concentration of anhydrous calcium chloride in the collagen solution is 0.05-0.2%, more preferably 0.05-0.1%, and further preferably 0.08-0.1%.
[0024] According to a specific embodiment of the present invention, the specific process of preparing the collagen solution is as follows: 0.5-15g collagen and 0.05-0.2g anhydrous calcium chloride (CaCl 2 ) add purified water to 100 ml to obtain anhydrous calcium chloride (CaCl 2) concentration of 0.5%-15% collagen solution; or without anhydrous calcium chloride (CaCl 2 ), add 0.5-15g collagen to 100ml of purified water to obtain a collagen solution with a concentration of 0.5%-15%.
[0025] According to a specific embodiment of the present invention, preferably, in step (2), the freeze-drying process comprises the following steps:
[0026] (1) Prefreezing: It is carried out in two stages. The process parameters of the first stage of prefreezing are that the temperature reaches 0-4°C from room temperature within 30-120 minutes and lasts for 30-180 minutes; the process parameters of the second stage of prefreezing are that the temperature reaches -60°C to -40°C within 60-180 minutes and lasts for 120-300 minutes;
[0027] (2) Sublimation: It is carried out in three stages. The process parameters of the first stage of sublimation are: within 30-120 minutes, the temperature reaches -30°C to -20°C, and lasts for 120-480 minutes, and the vacuum degree is 0.20-0.50 bar; the process parameters of the second stage of sublimation are: within 10-60 minutes, the temperature reaches -20°C to -15°C, and lasts for 120-480 minutes, and the vacuum degree is 0.10-0.20 bar; the process parameters of the third stage of sublimation are: within 10-60 minutes, the temperature reaches -15°C to -10°C, and lasts for 120-480 minutes, and the vacuum degree is 0.05-0.10 bar;
[0028] (3) Drying: within 60-180 minutes, the temperature reaches 20-40°C and lasts for 120-480 minutes, and the vacuum degree is 0.05-0.50;
[0029] The specific parameters are as follows:
[0030]
[0031] According to a specific embodiment of the present invention, preferably, in step (3), the dry heat cross-linking process comprises the following steps:
[0032] (1) placing the collagen sponge in a super-heat-conducting plate in a vacuum drying oven;
[0033] (2) The vacuum degree is set to -0.1 MPa to -0.05 MPa, the temperature is 100-220°C, and dry heat crosslinking is performed for 1-6 hours.
[0034] According to a specific embodiment of the present invention, preferably, during the dry heat crosslinking, the vacuum degree is -0.1 MPa to -0.08 MPa, more preferably -0.095 MPa to -0.09 MPa.
[0035] According to a specific embodiment of the present invention, preferably, during the dry heat crosslinking, the temperature is 150-220°C, more preferably 180-210°C.
[0036] According to a specific embodiment of the present invention, preferably, the dry heat cross-linking time is 2-5 hours, more preferably 3-4 hours.
[0037] According to a specific embodiment of the present invention, preferably, the equivalent thermal conductivity of the superconducting plate is 14MW / m·℃-30MW / m·℃, which is 32,000 times that of pure silver. For example, the superconducting plate is made of the superconducting heat transfer medium disclosed in CN1238721A.
[0038] The present invention performs dry heat crosslinking of materials on a superconducting plate and under vacuum conditions. The high temperature and extremely low or no oxygen content conditions used in the present invention can not only accelerate dehydration and enhance the interaction between molecular chains to achieve non-covalent crosslinking, but also form intermolecular crosslinking through esterification or amide, and at the same time, there is no influence of oxygen molecules, which can avoid the material from turning yellow and becoming brittle. The present invention adopts a superconducting plate based on inorganic thermal superconducting technology. The element has the characteristics of high-speed heat transfer, high heat transfer capacity, uniform temperature, small thermal resistance, and deformable structure. It is widely used in the fields of uniform temperature, heat dissipation, and heat exchange, and can replace traditional heat pipe technology; the present invention uses superconducting materials to prepare oven partitions. When heating, it can instantly heat up while ensuring that the temperature of each part is uniform, so that the collagen sponge is heated uniformly during the crosslinking process, which can greatly improve the quality and performance of the product itself, and at the same time significantly improve the yield rate (from 40%-50% to more than 95%). The present invention overcomes the prejudice of the prior art, can realize large-scale production, and ensures the uniform stability of the product itself and in large quantities. The material can be sterilized and crosslinked at the same time.
[0039] According to a specific embodiment of the present invention, preferably, the radiation cross-linking is cobalt 60 radiation cross-linking, which can initiate the formation and accumulation of covalent bonds between macromolecules in polymer linear molecules through radiation, and transform them into a three-dimensional network structure with a large molecular mass. Radiation cross-linking can greatly improve the cross-linking degree of the product, thereby significantly improving the mechanical properties, anti-degradation properties, flexibility, etc. of the product.
[0040] According to a specific embodiment of the present invention, preferably, the cross-linking dose of the radiation cross-linking is 20 kGy-35 kGy, more preferably 25 kGy-35 kGy, and further preferably 30 kGy-35 kGy.
[0041] The present invention also provides a double-layer collagen sponge, which is prepared by the above-mentioned preparation method.
[0042] According to a specific embodiment of the present invention, preferably, one side of the double-layer collagen sponge is a dense structure, and the other side is a loose structure.
[0043] According to a specific embodiment of the present invention, preferably, the thickness of the double-layer collagen sponge is 1-4 mm.
[0044] The present invention also provides application of the double-layer collagen sponge in preparing medical materials.
[0045] According to a specific embodiment of the present invention, preferably, the medical material is a hemostatic material, a repair material or a filling material used in oral and maxillofacial surgery, neurosurgery, general surgery or orthopedic medicine.
[0046] According to a specific embodiment of the present invention, preferably, the medical material is a hemostatic material, a repair material or a filling material for residual cavities used for trauma, burns and surgical wounds.
[0047] According to a specific embodiment of the present invention, the preparation method of the double-layer collagen sponge specifically comprises the following steps:
[0048] (1) Prepare collagen into a collagen solution and let it stand at room temperature to remove bubbles;
[0049] (2) adding the above collagen solution into a freeze-drying mold and performing vacuum freeze drying to obtain a collagen sponge with a three-dimensional structure;
[0050] (3) placing the collagen sponge into a superconducting plate of a superconducting electric vacuum drying oven, setting the vacuum degree to -0.1 MPa to -0.05 MPa, the temperature to 100°C to 220°C, and the cross-linking time to 1 h to 6 h; closing the door of the oven and starting to evacuate the air, and when the vacuum degree reaches the set range, the superconducting plate is instantly heated;
[0051] (4) performing radiation cross-linking to obtain the double-layer collagen sponge.
[0052] The collagen sponge provided by the present invention is based on an improved dry heat cross-linking technology and is obtained by adopting a physical double cross-linking technology, wherein the improved dry heat cross-linking technology is to perform dry heat cross-linking on a superconducting heat plate in a superconducting heat and electric heat vacuum drying box, and the obtained product has the following beneficial effects:
[0053] (1) The appearance and properties are better, the uniformity is better, and a double-layer collagen sponge consisting of a loose layer and a dense layer (i.e., a loose structure on one side and a dense structure on the other side) is obtained;
[0054] (2) Good intra-batch and inter-batch stability, high yield rate, good mechanical properties, soft and tough texture, and significantly improved mechanical properties, swelling properties, and anti-degradation properties;
[0055] (3) It also has good biocompatibility, is non-toxic, has no antigenic response, has low immunogenicity, and has controllable degradation;
[0056] (4) It has excellent adhesion, can effectively adhere to the application site, has good hemostatic effect, can be lightly pressed on the tissue wound surface during use, can adhere closely to the wound surface, absorb body fluids, mechanically seal blood vessel openings, and will not shift during human activities. It can be widely used in medical fields such as oral and maxillofacial surgery, neurosurgery, general surgery, and orthopedics, for example, for hemostasis, repair, and residual cavity filling of trauma, burns, and surgical wounds;
[0057] (5) The preparation process is simple, which greatly saves costs and shortens the production cycle. It is not only safe and effective, but also cheaper, with a high yield rate, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 This is a scanning electron microscope image of a recombinant collagen-like sponge with a three-dimensional structure after freeze-drying;
[0059] Figure 2 This is a scanning electron micrograph of the double-layer structure of a double-layer recombinant collagen-like sponge;
[0060] Figure 3 This is a scanning electron microscope image of the loose surface of a double-layer recombinant collagen sponge;
[0061] Figure 4 This is a scanning electron micrograph of the dense surface of a double-layer recombinant collagen-like sponge;
[0062] Figure 5 : are appearance pictures of collagen sponges, wherein (A) is the appearance picture of the recombinant collagen sponge of Comparative Example 1, and (B) is the appearance picture of the double-layer recombinant collagen sponge of Example 1;
[0063] Figure 6 This is a test chart of the mechanical properties and flexibility of the double-layer recombinant collagen sponge;
[0064] Figure 7 This is a test diagram of the adhesion of a double-layer recombinant collagen sponge;
[0065] Figure 8 This is a scanning electron micrograph of a single-layer recombinant collagen-like sponge;
[0066] Fig. 9 This is a diagram showing the cytotoxicity test results of a double-layer recombinant collagen sponge;
[0067] Fig.10 The results of HE staining sections of the double-layer recombinant collagen sponge after being embedded subcutaneously in SD rats for 2 weeks;
[0068] Fig.11 This is a test result of the blood absorption of double-layer recombinant collagen sponge;
[0069] Fig.12 This is a diagram showing the hemostatic effect of a blocky double-layer recombinant collagen sponge on rat liver;
[0070] Fig.13 The results of the comparison of the hemostatic effect of the double-layer recombinant collagen sponge and similar products on rat liver, where (A) is the 30s hemostatic structure and (B) is the 60s hemostatic result;
[0071] Fig.14 This is a comparison chart of the wound area sizes of each group when the double-layer recombinant collagen sponge was used to repair rat wounds 14 days ago. DETAILED DESCRIPTION
[0072] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0073] The superconducting heat-conducting plates used in the following examples were purchased from Huaqu Entropy Technology (Xi'an) Co., Ltd.
[0074] The recombinant collagen-like lyophilized powder used in the following examples is designed by optimizing the amino acid sequence, and a novel recombinant collagen-like protein is highly expressed by Pichia pastoris (see patent application publication text CN106554410A), and is obtained through large-scale fermentation and purification. Specifically, the hydrophilic Gly-XY repeat sequence is the minimum repeating unit of human type I collagen, and the novel collagen nucleotide sequence is designed by targeted arrangement and combination, and then the expression vector pPIC9K of Pichia pastoris is expressed in the Pichia pastoris host bacterium GS115 by electroporation. After screening with the antibiotic G418, the expression of the high-copy strain is expanded through the fermentation process, and the high-purity recombinant collagen-like protein is obtained by ultrafiltration and ion exchange chromatography purification.
[0075] Example 1
[0076] This embodiment provides a double-layer recombinant collagen sponge, which is prepared by the following steps:
[0077] Weigh 9 g of recombinant collagen freeze-dried powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A) and 0.18 g of anhydrous calcium chloride (CaCl 2 ), add 215.82g purified water, suspend evenly, and prepare 225ml containing 4% recombinant collagen and 0.08% anhydrous calcium chloride (CaCl 2) solution; the prepared solution was allowed to stand to remove bubbles and then added to a 3cm×5cm mold, with 4.5ml added to each mold; vacuum freeze-drying was performed to obtain 48 pieces of recombinant collagen sponges; the obtained recombinant collagen sponge was placed between superconducting plates in a superconducting electric vacuum drying oven, and the program was set to start vacuuming. When the vacuum degree reached the set value of -0.1MPa, the superconducting plate on which the product was placed was instantly heated to 180°C, and dry heat crosslinking was performed for 1h; the recombinant collagen sponge after dry heat crosslinking was sterilized by cobalt 60 irradiation at a sterilization dose of 30kGy to obtain the double-layer recombinant collagen sponge.
[0078] Among them, the freeze drying process is:
[0079] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 60 minutes and lasting for 300 minutes;
[0080] (2) Single sublimation drying: First, the vacuum degree is set to 0.30 mbar, and the temperature is increased from -50°C to -30°C within 30 minutes, and the temperature is maintained for 180 minutes; then the vacuum degree is set to 0.20 mbar, and the temperature is increased from -30°C to -15°C within 10 minutes, and the temperature is maintained for 360 minutes; finally, the vacuum degree is set to 0.10 mbar, and the temperature is increased from -15°C to -10°C within 10 minutes, and the temperature is maintained for 180 minutes;
[0081] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 40 min, and continued for 240 min.
[0082] The scanning electron microscope image of the double-layer recombinant collagen sponge is shown in Figure 1 As shown, it represents a recombinant collagen sponge with a three-dimensional structure after freeze-drying; the scanning electron microscopy image of the natural double-layer structure of the obtained double-layer recombinant collagen sponge is shown in Figure 2 The scanning electron microscope image of the loose surface of the obtained double-layer recombinant collagen sponge is shown in Figure 3 The scanning electron microscope image of the dense surface of the obtained double-layer recombinant collagen sponge is shown in Figure 4 As shown; the appearance of the double-layer recombinant collagen sponge is as follows Figure 5 As shown in B; the double-layer recombinant collagen sponge has good flexibility (such as Figure 6 As shown), good adhesion (as shown Figure 7 shown).
[0083] The cross-linking degree of the double-layer recombinant collagen sponge is shown in Table 1, and the inter-batch and intra-batch differences are much better than those of Comparative Examples 1 and 2; the finished product rate is shown in Table 2, which is much better than that of Comparative Examples 1 and 2.
[0084] Example 2
[0085] This embodiment provides a double-layer recombinant collagen sponge, which is prepared by the following steps:
[0086] Weigh 9g of recombinant collagen lyophilized powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A), add 216g of purified water, suspend evenly, and prepare 225ml of 4% recombinant collagen solution; let the above-prepared solution stand to remove bubbles, then add it to a 1cm×0.5cm×0.3cm mold, and add 150μl to each mold; perform vacuum freeze drying to obtain 1440 recombinant collagen sponges; place the obtained recombinant collagen sponge between superconducting plates in a superconducting electric vacuum drying oven, set the program to start vacuuming, and when the vacuum degree reaches the set value of -0.1MPa, the superconducting plate on which the product is placed is instantly heated to 200°C, and dry heat crosslinking is performed for 1h; the recombinant collagen sponge after dry heat crosslinking is sterilized by cobalt 60 irradiation, and the sterilization dose is 35kGy to obtain the double-layer recombinant collagen sponge.
[0087] Among them, the freeze drying process is:
[0088] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 40 minutes and lasting for 300 minutes;
[0089] (2) Single sublimation drying: First, the vacuum degree is set to 0.30 mbar, and the temperature is increased from -50°C to -30°C within 30 minutes, and the temperature is maintained for 180 minutes; then the vacuum degree is set to 0.20 mbar, and the temperature is increased from -30°C to -15°C within 30 minutes, and the temperature is maintained for 360 minutes; finally, the vacuum degree is set to 0.10 mbar, and the temperature is increased from -15°C to -10°C within 30 minutes, and the temperature is maintained for 180 minutes;
[0090] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 60 min, and continued for 240 min.
[0091] The results of the in vivo hemostasis experiment of the double-layer recombinant collagen sponge are shown in Table 8. In Example 1, anhydrous calcium chloride (CaCl 2 The hemostasis time of the double-layer recombinant collagen sponge was significantly longer than that of Example 2 without the addition of anhydrous calcium chloride (CaCl 2 ) of the recombinant collagen sponge had a short hemostasis time, indicating that the addition of anhydrous calcium chloride (CaCl 2 ) can increase the rate of hemostasis.
[0092] Example 3
[0093] This embodiment provides a double-layer recombinant collagen sponge, which is prepared by the following steps:
[0094] Weigh 11.25 g of recombinant collagen freeze-dried powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A) and 0.225 g of anhydrous calcium chloride (CaCl 2 ), add 213.53 g purified water, suspend evenly, and prepare 225 ml containing 5% recombinant collagen and 0.1% anhydrous calcium chloride (CaCl 2 ) solution; the prepared solution was allowed to stand to remove bubbles and then added to a 3cm×5cm mold, with 4.5ml added to each mold; vacuum freeze-drying was performed to obtain 48 pieces of recombinant collagen sponges; the obtained recombinant collagen sponge was placed between superconducting plates in a superconducting electric vacuum drying oven, and the program was set to start vacuuming. When the vacuum degree reached the set value of -0.1MPa, the superconducting plate on which the product was placed was instantly heated to 200°C, and dry heat crosslinking was performed for 2h; the recombinant collagen sponge after dry heat crosslinking was sterilized by cobalt 60 irradiation at a sterilization dose of 30kGy to obtain the double-layer recombinant collagen sponge.
[0095] Among them, the freeze drying process is:
[0096] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 60 minutes and lasting for 300 minutes;
[0097] (2) Single sublimation drying: First, the vacuum degree is set to 0.30 mbar, and the temperature is increased from -50°C to -30°C within 30 minutes, and the temperature is maintained for 180 minutes; then the vacuum degree is set to 0.20 mbar, and the temperature is increased from -30°C to -15°C within 10 minutes, and the temperature is maintained for 360 minutes; finally, the vacuum degree is set to 0.10 mbar, and the temperature is increased from -15°C to -10°C within 10 minutes, and the temperature is maintained for 180 minutes;
[0098] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 40 min, and continued for 240 min.
[0099] Example 4
[0100] This embodiment provides a double-layer recombinant collagen sponge, which is prepared by the following steps:
[0101] Weigh 13.5 g of recombinant collagen freeze-dried powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A) and 0.225 g of anhydrous calcium chloride (CaCl2 ), add 211.28g purified water, suspend evenly, and prepare 225ml containing 6% recombinant collagen and 0.1% anhydrous calcium chloride (CaCl 2 ) solution; the prepared solution was allowed to stand to remove bubbles and then added to a 3cm×5cm mold, with 4.5ml added to each mold; vacuum freeze-drying was performed to obtain 48 pieces of recombinant collagen sponges; the obtained recombinant collagen sponge was placed between superconducting plates in a superconducting electric vacuum drying oven, and the program was set to start vacuuming. When the vacuum degree reached the set value of -0.1MPa, the superconducting plate on which the product was placed was instantly heated to 210°C, and dry heat crosslinking was performed for 2h; the recombinant collagen sponge after dry heat crosslinking was sterilized by cobalt 60 irradiation at a sterilization dose of 35kGy to obtain the double-layer recombinant collagen sponge.
[0102] Among them, the freeze drying process is:
[0103] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 60 minutes and lasting for 300 minutes;
[0104] (2) Single sublimation drying: First, the vacuum degree was set to 0.25 mbar, and the temperature was increased from -50°C to -30°C within 30 min, and continued for 180 min; then the vacuum degree was set to 0.15 mbar, and the temperature was increased from -30°C to -15°C within 10 min, and continued for 360 min; finally, the vacuum degree was set to 0.10 mbar, and the temperature was increased from -15°C to -10°C within 10 min, and continued for 240 min;
[0105] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 60 min, and continued for 240 min.
[0106] Comparative Example 1
[0107] This comparative example provides a recombinant collagen sponge, which is prepared by the following steps:
[0108] Weigh 9 g of recombinant collagen freeze-dried powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A) and 0.18 g of anhydrous calcium chloride (CaCl 2 ), add 215.82g purified water, suspend evenly, and prepare 225ml containing 4% recombinant collagen and 0.08% anhydrous calcium chloride (CaCl 2) solution; the prepared solution was allowed to stand to remove bubbles and then added to a 3cm×5cm mold, with 4.5 ml added to each mold; vacuum freeze-drying was performed to obtain 48 samples; the obtained samples were placed in a blast drying oven, heated to 180°C, and dry-heat cross-linked for 1h after the temperature reached 180°C; the dry-heat cross-linked samples were sterilized by cobalt 60 irradiation at a sterilization dose of 35kGy to obtain the recombinant collagen sponge.
[0109] Among them, the freeze drying process is:
[0110] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 60 minutes and lasting for 300 minutes;
[0111] (2) Single sublimation drying: First, the vacuum degree is set to 0.30 mbar, and the temperature is increased from -50°C to -30°C within 30 minutes, and the temperature is maintained for 180 minutes; then the vacuum degree is set to 0.20 mbar, and the temperature is increased from -30°C to -15°C within 10 minutes, and the temperature is maintained for 360 minutes; finally, the vacuum degree is set to 0.10 mbar, and the temperature is increased from -15°C to -10°C within 10 minutes, and the temperature is maintained for 180 minutes;
[0112] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 40 min, and continued for 240 min.
[0113] The appearance of the recombinant collagen sponge is Figure 5 As shown in A, if the oxygen content is too high or the temperature is too high during the cross-linking process, carbonization will occur, the appearance will be brown-yellow, there will be no toughness, and the brittleness will increase accordingly; the degree of cross-linking is shown in Table 1, and the inter-batch and intra-batch differences are worse than those of Comparative Example 2 and Example 1; the yield rate is shown in Table 2, which is worse than that of Comparative Example 2 and Example 1.
[0114] Comparative Example 2
[0115] This comparative example provides a recombinant collagen sponge, which is prepared by the following steps:
[0116] Weigh 9g of recombinant collagen lyophilized powder (the recombinant human collagen obtained in Example 1 of patent application publication CN106554410A), add 216g of purified water, suspend evenly, and prepare 225ml of 4% recombinant collagen solution; let the above-prepared solution stand to remove bubbles, then add it to a 3cm×5cm mold, and add 4.5ml to each mold; perform vacuum freeze drying to obtain 48 samples; place the obtained samples in an ordinary vacuum drying oven, set the vacuum degree to -0.1MPa, and the dry heat crosslinking temperature to 200°C. After the temperature reaches the set 200°C, perform dry heat crosslinking for 1h; sterilize the dry heat crosslinked samples by cobalt 60 irradiation with a sterilization dose of 35kGy to obtain the recombinant collagen sponge.
[0117] Among them, the freeze drying process is:
[0118] (1) Pre-freezing stage 1: from room temperature to 0°C within 30 minutes and lasting for 60 minutes; pre-freezing stage 2: from 0°C to -50°C within 40 minutes and lasting for 300 minutes;
[0119] (2) Single sublimation drying: First, the vacuum degree is set to 0.30 mbar, and the temperature is increased from -50°C to -30°C within 30 minutes, and the temperature is maintained for 180 minutes; then the vacuum degree is set to 0.20 mbar, and the temperature is increased from -30°C to -15°C within 30 minutes, and the temperature is maintained for 360 minutes; finally, the vacuum degree is set to 0.10 mbar, and the temperature is increased from -15°C to -10°C within 30 minutes, and the temperature is maintained for 180 minutes;
[0120] (3) Desorption drying: The vacuum degree was set to 0.10 mbar, the temperature reached 30 °C within 60 min, and continued for 240 min.
[0121] Comparative Example 3
[0122] This comparative example provides a recombinant collagen sponge, which is prepared by the following steps:
[0123] Weigh 9 g of recombinant collagen freeze-dried powder (recombinant human collagen obtained in Example 1 of patent application publication CN106554410A) and 0.18 g of anhydrous calcium chloride (CaCl 2 ), add 215.82g purified water, suspend evenly, and prepare 225ml containing 4% recombinant collagen and 0.08% anhydrous calcium chloride (CaCl 2) solution; the prepared solution was allowed to stand to remove bubbles and then added to a 3cm×5cm mold, 4.5ml was added to each mold; vacuum freeze drying was performed once; cross-linking agent was prepared: 9.2g of 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC) was weighed and added to 960.0g of purified water, and the mixture was thoroughly mixed and dissolved; the prepared cross-linking agent was poured into a cross-linking disk, and a freeze-dried sample was immersed in the cross-linking agent, and cross-linked at 50-80r / min for 24h in a shaker at 37°C; the cross-linked sample was taken out and placed in a cleaning mold, 10L of purified water at a temperature of 25-35°C was added, the cleaning disk was placed in a shaker, and the cleaning was vibrated and cleaned for 1h at a speed of 50-80r / min, the cleaning water was discarded, and the cleaning was repeated according to the above cleaning steps, and the cleaning was repeated for a total of 24h before freeze drying again to obtain 48 recombinant collagen sponges, wherein the two freeze-drying processes were the same as those in Example 1.
[0124] The obtained recombinant collagen sponge is a single-layer structure, such as Figure 8 shown.
[0125] The products obtained in Example 1, Comparative Example 1 and Comparative Example 2 were subjected to relevant performance tests, as follows:
[0126] Appearance: Observed with naked eyes under fluorescent light, the appearance of Comparative Example 1 is yellow or light yellow, and the color is uneven; Comparative Example 2 is no different from Example 1, both are uniformly white.
[0127] Determination of cross-linking degree: The reaction between trinitrobenzenesulfuric acid (TNBS) and amino acid functional groups is used to measure the number of free amino groups in the cross-linked collagen matrix by detecting the ultraviolet absorption light value, and the change in the number of free amino groups reflects the cross-linking degree of the product. In simple terms, the number of free amino groups is inversely proportional to the cross-linking degree. The more free amino groups, the lower the cross-linking degree. The specific scheme is: accurately weigh about 5 mg of the sample, place it in a 25 mL stoppered test tube, add 1 mL of 4% sodium bicarbonate solution and 1 mL of 0.5% TNBS solution, and heat it in a 40°C water bath for 2 hours. Add 3 mL of 6 mol / L HCl solution, place it in an autoclave and heat it at 120°C for 30 minutes, dilute the resulting solution with 5 mL of water, extract it with ether 3 times, 10 mL each time, discard the ether layer, absorb 5 mL of the aqueous phase, heat it in a boiling water bath for 15 minutes, cool it to room temperature, dilute it with water, shake it well, and measure the absorbance at a wavelength of 346 nm.
[0128] Cross-linking degree (%) = 1 - (absorbance value of cross-linked sample / mass of cross-linked sample) / (absorbance value of non-cross-linked sample / mass of non-cross-linked sample).
[0129] Table 1
[0130]
[0131] The results are shown in Table 1. The crosslinking degree of the product in Example 1 is significantly improved compared with that in Comparative Examples 1 and 2, and the inter-batch and intra-batch differences are significantly reduced.
[0132] Yield rate: As shown in Table 2, the yield rate of Example 1 is significantly improved compared with Comparative Examples 1 and 2.
[0133] Table 2
[0134]
[0135] Mechanical properties test: According to GB / T 3923.1-1997 Part 1: Determination of breaking strength and breaking elongation (strip method), the samples were cut into 0.5 mm × 5 mm and the tensile breaking strength and breaking elongation tests were carried out using a single-column electronic universal testing machine. The results are shown in Table 3. The mechanical properties of Example 1 are significantly better than those of Comparative Examples 1 and 2.
[0136] Table 3
[0137]
[0138] Swelling determination: Use a vernier caliper to measure the actual size V of each group of samples 0 , and then weigh its initial weight (w 0 ), record the data, soak the sample in distilled water for 0.5h, take it out and use filter paper to absorb the moisture on the surface of the sample, weigh it (w), and use a vernier caliper to measure the size V after water absorption and expansion. Swelling rate (%) = ((ww o ) / w o )×100%, volume ratio before and after swelling = V / V 0 As shown in Table 4, the swelling property of Example 1 is significantly better than that of Comparative Examples 1 and 2.
[0139] Table 4
[0140]
[0141] In vitro degradation determination: The sample was made into a disc with a diameter of 1 cm using a puncher, and then the disc and type I collagenase solution (20 units / mL) were added to a sterile centrifuge tube, and the degradation rates of Example 1, Comparative Example 1 and Comparative Example 2 were calculated by constant weight method under constant temperature of 37°C for 30 minutes. The results are shown in Table 5. After 30 minutes of degradation, the in vitro degradation rate of Example 1 was significantly lower than that of Comparative Example 1 and Comparative Example 2.
[0142] Table 5
[0143]
[0144] In summary: after dry heat crosslinking in a superconducting heat electric vacuum drying oven, the surface and internal crosslinking degree of the sample is more uniform, the overall crosslinking degree is better, the mechanical properties are better, the anti-degradation time is longer, and the swelling property is significantly improved. The swelling property is generally inversely proportional to the crosslinking degree.
[0145] Cytotoxicity assay: According to GB / T 16886.5-2017 Biological Evaluation of Medical Devices Part 5: In vitro Cytotoxicity Test MTT method, the double-layer recombinant collagen sponge obtained in Example 1 was subjected to cytotoxicity test (two parallel experiments were conducted, and both Sample 1 and Sample 2 were the products obtained in Example 1). The specific operation was as follows: using high-glucose DMEM culture medium as the extraction medium, first the recombinant collagen sponge was thoroughly swollen, and then extracted at a ratio of 0.1 g / ml, the extraction temperature was 37°C, and the extraction time was 24 h; the L929 cells that were vigorously growing for 48-72 h were trypsinized and collected, and the high-glucose DMEM culture medium was used to prepare the cell concentration to 1×10 7 L -1 The cell suspension was inoculated into a 96-well plate, 200 μL per well. 200 μL of cell suspension was added to each well of the 96-well plate. After changing the medium the next day, 200 μL of recombinant collagen sponge extract was added to the experimental group, the negative control group (NC) was added with conventional culture medium, the positive control group (PC) was added with 5% DMSO, and the blank control group (BC) was an extraction medium without the sample, that is, high-glucose DMEM culture medium. At the 68th hour of culture, 20 μL of MTT reagent was added to each well, incubated in a cell culture incubator for 4 hours, the liquid was discarded, 160 μL of DMSO was added to each well, and 160 μL of DMSO was also added to the zeroing well at this time, and low-speed shaking was performed for 10 minutes. The absorbance value (OD value) of each well was measured at a wavelength of 490 nm using an enzyme-linked immunosorbent assay, and the absorbance value of the blank zeroing well was zeroed, and the average value was taken and recorded.
[0146] The relative proliferation rate of cells was calculated according to the following formula based on the mean absorbance of each group: relative proliferation rate of cells = average absorbance value of experimental group / average absorbance value of negative control group × 100%. When the relative proliferation rate of cells is ≥100%, the cytotoxicity is level 0; when the relative proliferation rate of cells is between 80%-99%, the cytotoxicity is level 1; when the relative proliferation rate of cells is between 50%-79%, the cytotoxicity is level 2; when the relative proliferation rate of cells is between 30%-49%, the cytotoxicity is level 3; when the relative proliferation rate of cells is between 0-29%, the cytotoxicity is level 4. The experimental results are shown in Table 6 and Fig. 9 shown.
[0147] Table 6
[0148]
[0149]
[0150] As can be seen from Table 6, the recombinant collagen sponge of the present invention has good biocompatibility and no cytotoxicity.
[0151] Subcutaneous embedding experiment of SD rats: The double-layer recombinant collagen sponge obtained in Example 1 was subjected to subcutaneous embedding experiment. The specific operation was as follows: SD rats were purchased and brought to the laboratory to adapt to the environment for one week; anesthetized and skin prepared, intraperitoneal anesthesia was performed with 3% sodium pentobarbital, and the anesthetic dose was 30 mg / kg. After successful anesthesia, the back was shaved with electric clippers, the skin of the rat was cut open with surgical scissors, and the double-layer recombinant collagen sponge material (1 cm×1 cm) was placed in it, and the wound was sutured. After 1 week, 2 weeks, and 3 weeks, the samples were observed and taken, and 10% formaldehyde was used for fixation and HE staining and sectioning. The results of 3 weeks are as follows. Fig.10 As can be seen from the figure, there are fewer inflammatory cells, tissues and materials grow in an interlaced manner, and most tissues and cells migrate into the material. It can be seen that the recombinant collagen sponge of the present invention has low immunogenicity and good biocompatibility.
[0152] Blood-sucking, hemostasis and wound repair effects:
[0153] The double-layer recombinant collagen sponge obtained in Example 1 was subjected to an in vitro blood absorption experiment. The specific operation was as follows: the sample was cut into 1 cm×1 cm pieces; 10 ml of fresh rabbit blood was taken, and 1 ml of anticoagulant (1 g / L heparin aqueous solution) was added; 5 ml of rabbit blood was drawn with a 10 ml syringe and dripped onto the sample surface quickly and uniformly; a stopwatch was used to record the complete blood absorption time and the blood absorption amount when complete blood absorption occurred. The results are shown in Table 7 and Table 8. Fig.11 As shown, it can be seen that the recombinant collagen sponge has good blood absorption ability.
[0154] At the same time, the block and sheet double-layer recombinant collagen sponge obtained in Example 1 was compared with similar products in rat liver hemostasis effect. The specific operation was to conduct two identical wound bleeding tests on the liver of the same rat, and use recombinant collagen and natural collagen sponges for hemostasis respectively. The observation time was 30s, and the results were as follows: Fig.12 (Example 1 Block-shaped double-layer recombinant collagen sponge) and Fig.13 , it can be seen that the control group did not completely stop bleeding, while the experimental group completely stopped bleeding ( Fig.13 Middle A); 60s results showed that both groups had complete hemostasis ( Fig.13 (B), the in vivo hemostasis time results of the double-layer recombinant collagen sponges obtained in Example 1 and Example 2 are shown in Table 8.
[0155] In addition, the recombinant collagen sponge obtained in Example 1 was used to repair wounds in SD rats. The specific plan was as follows: SD rats were purchased and brought to the laboratory to adapt to the environment for one week. Anesthetized and skin prepared, intraperitoneal anesthesia was performed with 3% sodium pentobarbital, and the anesthetic dose was 30 mg / kg. After successful anesthesia, the back was shaved with electric clippers. A circular full-thickness skin excision wound with a diameter of 7 mm was made on the back of the animal using a skin sampler (7 mm in diameter) for modeling, and marked with India ink. The wounds of the experimental group, control group, and blank group corresponded to the recombinant collagen sponge group, natural collagen group, and blank control group in Example 1, respectively. After the model was established, it was covered with the corresponding sponge, and the image-pro-plus software was used to measure the size of the wound repair. The results are shown in the figure. Fig.14 As shown (vertical axis unit: AOI value), the wound area size results of each group when the sample was taken on the 14th day were compared, indicating that the recombinant collagen sponge of the present application has the effect of promoting wound healing.
[0156] Table 7
[0157]
[0158] Table 8
[0159]
[0160] In summary, the above are only preferred embodiments of the present invention, and are not intended to limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a double-layer collagen sponge, comprising the following steps: (1) preparing collagen into a collagen solution; (2) freeze-drying the collagen solution to obtain a collagen sponge; (3) subjecting the collagen sponge to dry heat crosslinking and radiation crosslinking under vacuum conditions to obtain the double-layer collagen sponge; Wherein, in step (3), dry heat crosslinking is carried out on a super heat conducting plate in a vacuum drying oven.
2. The preparation method according to claim 1, wherein In step (1), the collagen is recombinant collagen; Preferably, the recombinant collagen is the recombinant human collagen disclosed in CN106554410A; Preferably, the concentration of collagen in the collagen solution is 0.5-15%, more preferably 1-10%.
3. The preparation method according to claim 1, wherein In step (1), the composition of the collagen solution also includes an inorganic calcium salt, and the inorganic calcium salt is preferably anhydrous calcium chloride; Preferably, the concentration of anhydrous calcium chloride in the collagen solution is 0.05-0.2%, more preferably 0.05-0.1%.
4. The preparation method according to claim 1, wherein In step (2), the freeze-drying process comprises the following steps: (1) Prefreezing: It is carried out in two stages. The process parameters of the first stage of prefreezing are that the temperature reaches 0-4°C from room temperature within 30-120 minutes and lasts for 30-180 minutes; the process parameters of the second stage of prefreezing are that the temperature reaches -60°C to -40°C within 60-180 minutes and lasts for 120-300 minutes; (2) Sublimation: It is carried out in three stages. The process parameters of the first stage of sublimation are: within 30-120 minutes, the temperature reaches -30°C to -20°C, and lasts for 120-480 minutes, and the vacuum degree is 0.20-0.50 bar; the process parameters of the second stage of sublimation are: within 10-60 minutes, the temperature reaches -20°C to -15°C, and lasts for 120-480 minutes, and the vacuum degree is 0.10-0.20 bar; the process parameters of the third stage of sublimation are: within 10-60 minutes, the temperature reaches -15°C to -10°C, and lasts for 120-480 minutes, and the vacuum degree is 0.05-0.10 bar; (3) Analytical drying: within 60-180 minutes, the temperature reaches 20-40°C and lasts for 120-480 minutes, with a vacuum degree of 0.05-0.
50.
5. The preparation method according to claim 1, wherein In step (3), the dry heat cross-linking process comprises the following steps: (1) placing the collagen sponge in a superheat-conducting plate in a vacuum drying oven; (2) the vacuum degree is set to -0.1 MPa to -0.05 MPa, the temperature is 100-220°C, and dry heat crosslinking is performed for 1-6 hours; Preferably, during dry heat crosslinking, the vacuum degree is -0.1 MPa to -0.08 MPa; Preferably, during dry heat crosslinking, the temperature is 150-220°C; Preferably, the dry heat crosslinking time is 2-5 hours.
6. The preparation method according to claim 5, wherein: The equivalent thermal conductivity of the superconducting plate is 14MW / m·℃-30MW / m·℃.
7. The preparation method according to claim 1, wherein The radiation cross-linking is cobalt 60 radiation cross-linking; Preferably, the crosslinking dose of the radiation crosslinking is 20 kGy-35 kGy, more preferably 25 kGy-35 kGy.
8. A double-layer collagen sponge, prepared by the preparation method according to any one of claims 1 to 7; Preferably, one side of the double-layer collagen sponge is a dense structure, and the other side is a loose structure; Preferably, the thickness of the double-layer collagen sponge is 1-4 mm.
9. Use of the double-layer collagen sponge according to claim 8 in the preparation of medical materials.
10. The use according to claim 9, wherein: The medical material is a hemostatic material, a repair material or a filling material used in oral and maxillofacial surgery, neurosurgery, general surgery or orthopedics; Preferably, the medical material is a hemostatic material, a repair material or a filling material for residual cavities used for trauma, burns and surgical wounds.
Citation Information
Patent Citations
Recombinant human collagen and its coding gene and preparation method thereof
CN106554410A
Recombinant collagen protein, recombinant collagen sponge material as well as preparation method and application of recombinant collagen sponge material
CN111187347A
Super conducting heat transfer medium
CN1238721A
Cited By
Recombinant collagen and application thereof, collagen sponge and preparation method and application thereof
CN119823258A
Performance-enhanced collagen sponge and preparation method thereof
CN119909221A