Polymer-based wear-resistant composite material filled with core-shell particles and preparation method of polymer-based wear-resistant composite material

By using core-shell particle fillers composed of graphene and nanometal particles in polymer-based composite materials, the problem of difficulty in uniform dispersion of various fillers at high contents is solved, and friction performance and wear resistance can be improved at low contents, and Reduced costs.

CN118772487AActive Publication Date: 2024-10-15JILIN UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411003237.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-15
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In polymer-based composite materials, although the introduction of various fillers can improve friction properties, high-content fillers are difficult to disperse evenly, resulting in limited improvement in mechanical properties and friction properties and high costs.

Method used

Using core-shell particle fillers, the shell is graphene, and the central core is nanometal particles. By heating the β-diketone metal complex under vacuum conditions and passing in reducing gas for insulation, a diameter of 100nm-300nm is prepared. The nano-core-shell particle filler is uniformly mixed with the polymer matrix, and the composite material is prepared by molding.

Benefits of technology

At a lower content, it significantly improves the friction performance of composite materials, has good wear resistance and self-lubricating properties, solves the problem of poor filler dispersion, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118772487A_ABST
    Figure CN118772487A_ABST
Patent Text Reader

Abstract

The invention provides a core-shell particle filled polymer-based wear-resistant composite material and a preparation method thereof, and belongs to the technical field of polymer-based wear-resistant composite materials. According to the core-shell particle filler provided by the invention, a shell is graphene, and a central core is nano metal particles; and the diameter of the core-shell particle filler is 100 nm to 300 nm. And compounding the core-shell particle filler with a polymer matrix to obtain the core-shell particle filled polymer-based wear-resistant composite material. The core-shell particle filler can be used as a solid lubricant in a polymer-based composite material, can well improve the friction performance of the composite material at a low content, has good wear resistance and self-lubrication, can effectively solve the problem of dispersion of the filler in a matrix, and reduces the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer-based wear-resistant composite materials, and in particular to a polymer-based wear-resistant composite material filled with core-shell particles and a preparation method thereof. Background Art

[0002] Engineering plastics refer to a type of polymer material that can be used as a structural material, withstand mechanical stress in a wide temperature range, and be used in a harsh chemical and physical environment. Engineering plastics can be divided into two categories: general engineering plastics and special engineering plastics. The former mainly includes polyamide, polyoxymethylene, polyphenylene ether, etc.; the latter mainly refers to engineering plastics with a long-term use temperature above 150°C, and the main varieties include polyimide, polysulfone, polyphenylene sulfide, polytetrafluoroethylene, polyetheretherketone, etc. Engineering plastics have a wide range of applications due to their excellent stability, good heat and chemical resistance, and high strength, and their demand continues to grow rapidly. One of the main uses of engineering plastics is to replace metals in the application of wear-resistant materials. Compared with metal materials, engineering plastics are light in weight, high in specific strength, easy to process, high in production efficiency, and have outstanding friction reduction and wear resistance. With the technical requirements of modern high-end equipment for system reliability and long life, a single engineering plastic often cannot simultaneously meet the system's requirements for material self-lubricity and wear resistance, so it is necessary to fill and modify engineering plastic materials to meet a wider range of application needs.

[0003] At present, the filler-modified fillers commonly used by researchers to improve the tribological properties of polymers are mainly the following: metal and compound fillers such as copper, lead, tin, etc.; inorganic fillers such as carbon fiber, molybdenum disulfide, graphite, etc.; nanofillers such as nanoalumina, graphene, carbon nanotubes, etc. Filling a single filler to improve the friction performance of polymers is often not enough to meet the performance requirements, and the introduction of multiple fillers can give full play to the functions of the fillers. On the basis of maintaining the original advantages of the polymer matrix, the synergistic and complementary effects of multiple components are fully utilized, thereby improving and overcoming the defects of the polymer matrix and achieving the best comprehensive performance, thereby further improving the friction performance of the polymer. Yongwu Zhao et al. (Materials, 2022, 15, 7078) studied the friction performance of polyetheretherketone / polytetrafluoroethylene composites enhanced by adding carbon fiber and graphite. The study showed that the synergistic effect of carbon fiber and graphite can effectively improve the wear resistance of the composite material. However, there are still some shortcomings in the practical application of multi-component modified polymer-based composites. The content of various fillers in the composites is often very high, and some high-content fillers are easy to agglomerate and difficult to disperse evenly in the matrix, which will be detrimental to the improvement of the mechanical properties and friction properties of the composites. Summary of the invention

[0004] To solve the above problems, the present invention provides a core-shell particle filled polymer-based wear-resistant composite material and a preparation method thereof. The core-shell particle filler in the present invention can be used as a solid lubricant in the polymer-based composite material, can well improve the friction properties of the composite material at a lower content, has good wear resistance and self-lubricating properties, can effectively solve the dispersion problem of the filler in the matrix, and reduce costs.

[0005] In order to achieve the above object, the present invention provides the following technical solution: a core-shell particle filler, wherein the shell is graphene and the central core is a nano metal particle; the diameter of the core-shell particle filler is 100nm-300nm.

[0006] Preferably, the nano metal particles include Cu, Ag, Zn, Sn or Al.

[0007] The present invention also provides a method for preparing the core-shell particle filler, which comprises heating the β-diketone metal complex under vacuum conditions, introducing a reducing gas to keep the temperature to reduce the β-diketone metal complex, and obtaining the core-shell particle filler;

[0008] The structural formula of the β-diketone metal complex is: wherein R1 and R2 are each independently selected from CH3-, C2H5-, n-C3H7-, i-CH3, n-C4H9-, i-C4H9-, s-C4H9-, t-C4H9-, CH3O-, C2H5O-, Ph-, p-CH3-Ph-, p-C2H5-Ph-, p-CH3O-Ph- or p-C2H5O-Ph-; M n+ Cu 2+ 、Ag + 、Zn 2+ Sn 2+ or Al 3+ .

[0009] Preferably, the vacuum condition is a vacuum degree ≤ 60Pa.

[0010] Preferably, the β-diketone metal complex is heated to 450-600° C. and the insulation time is 150-200 minutes.

[0011] Preferably, the reducing gas comprises CO or H2.

[0012] The invention also provides application of the core-shell particle filler in preparing polymer-based composite materials.

[0013] The invention also provides a polymer-based wear-resistant composite material filled with core-shell particles, the raw materials of which include a polymer and the core-shell particle filler.

[0014] Preferably, the polymer is polyetheretherketone, polyphenylene sulfide, polyimide, polyetherimide, nylon 66 or polyoxymethylene.

[0015] The present invention also provides a method for preparing the core-shell particle filled polymer-based wear-resistant composite material, wherein the core-shell particle filler is uniformly mixed with a polymer, and then compression molding is performed to obtain the core-shell particle filled polymer-based composite material.

[0016] The present invention discloses the following technical effects:

[0017] 1. The shell of the nano core-shell particle filler provided by the present invention is composed of layered graphene, and the core is a metal nanoparticle. The two-dimensional graphene sheets are connected by van der Waals forces, and the low shear force between adjacent atomic layers makes the atomic layers easy to slide, thus giving it lubrication properties. In addition, due to the nanostructure of the core-shell particles, it is easy to enter the friction contact surface to form a lubricating film, which can reduce surface roughness and repair wear.

[0018] 2. The nano core-shell particle filler provided by the present invention can be used as a solid lubricant for a variety of engineering plastics to improve the friction performance of engineering plastics, and is not limited to being used as a lubricant additive. The core-shell particles of the present invention combine graphene with metal nanoparticles, which solves the limitation of improving friction performance brought by a single filler, and solves the problem of large dosage and poor dispersibility of existing multiple fillers.

[0019] 3. The present invention uses core-shell particle fillers as solid lubricants and composites them with polymer matrices to prepare composite materials. When friction occurs, the core-shell particles are peeled off, and the outer flaky graphene is peeled off from the surface of the core-shell particles to form a transfer film together with the peeled polymer matrix; the exposed metal nanoparticles roll on the friction interface, playing the role of "nano bearings" and enhancing the shear resistance of the transfer film; at the same time, the metal nanoparticles induce friction chemical reactions during the friction process, and the chemical reaction is conducive to the formation of a high-quality transfer film.

[0020] 4. Low content of core-shell particle filler can effectively improve the friction performance of the composite material, solve the problem of poor dispersibility, and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is the SEM image of the core-shell particles obtained in Example 1. DETAILED DESCRIPTION

[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0024] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0025] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0026] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0027] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0028] The invention provides a core-shell particle filler, wherein the shell is graphene and the central core is a nano metal particle; the diameter of the core-shell particle filler is 100nm-300nm.

[0029] In some embodiments, the nanometal particles include Cu, Ag, Zn, Sn or Al.

[0030] The present invention also provides a method for preparing the core-shell particle filler, which comprises heating the β-diketone metal complex under vacuum conditions, introducing a reducing gas to keep the temperature to reduce the β-diketone metal complex, and obtaining the core-shell particle filler;

[0031] The structural formula of the β-diketone metal complex is: wherein R1 and R2 are each independently selected from CH3-, C2H5-, n-C3H7-, i-CH3, n-C4H9-, i-C4H9-, s-C4H9-, t-C4H9-, CH3O-, C2H5O-, Ph-, p-CH3-Ph-, p-C2H5-Ph-, p-CH3O-Ph- or p-C2H5O-Ph-; M n+ Cu 2+ 、Ag + 、Zn 2+ Sn 2+ or Al 3+ .

[0032] In some embodiments, the vacuum condition is a vacuum degree ≤ 60Pa.

[0033] In some embodiments, the β-diketone metal complex is heated to 450-600° C. and the insulation time is 150-200 minutes.

[0034] In some embodiments, the temperature for heating the β-diketone metal complex is 550° C. and the insulation time is 180 minutes.

[0035] In some embodiments, the reducing gas comprises CO or H2.

[0036] In some embodiments, the reducing gas is H2.

[0037] In some embodiments, after introducing reducing gas to keep warm to reduce the acetylacetone metal complex, the present invention further includes the steps of naturally cooling to room temperature, washing, centrifuging, and drying.

[0038] In some embodiments, the washing is to use an organic solvent to wash away the unreacted acetylacetone metal complex in the product; the organic solvent is chloroform, benzene, carbon tetrachloride, ether, methanol, ethanol, isopropanol, n-butanol, dimethyl sulfoxide, ethyl acetate, acetone, butanone, pyridine or tetrahydrofuran, preferably ethanol, acetone or ethyl acetate.

[0039] The invention also provides application of the core-shell particle filler in preparing polymer-based composite materials.

[0040] The invention also provides a polymer-based wear-resistant composite material filled with core-shell particles, the raw materials of which include a polymer and the core-shell particle filler.

[0041] In some embodiments, the polymer is polyetheretherketone, polyphenylene sulfide, polyimide, polyetherimide, nylon 66 or polyoxymethylene; and the particle size of the polymer is less than 100 μm.

[0042] The present invention does not specifically limit the type of the polymer, and any commercially available product that meets the above-mentioned particle size can be used. The polymers within the scope of the present invention are engineering plastics and special engineering plastics commonly used for friction reduction. However, in view of the different technical requirements of modern high-end equipment for materials, other polymer materials can also be tried in the scheme of the present invention to meet the needs of widespread use of friction materials in various fields.

[0043] In some embodiments, the mass ratio of the core-shell particle filler to the polymer is (2-20):80.

[0044] The mass ratio of core-shell particles to polymer set in the present invention is (2-20):80. Within this range, the mass fraction of the filler is less than 20%, which is conducive to a more uniform dispersion of the filler in the matrix, and the friction performance of the composite material reinforced with a low content of filler is significantly improved. If the mass fraction of the filler is higher than 20%, the filler will be unevenly dispersed in the polymer matrix, agglomeration will occur, and the friction performance of the composite material reinforced with a high content of filler is not significantly improved compared to the composite material filled with a low content of filler, and may even be reduced.

[0045] The present invention also provides a method for preparing the core-shell particle filled polymer-based wear-resistant composite material, wherein the core-shell particle filler is uniformly mixed with a polymer, and then compression molding is performed to obtain the core-shell particle filled polymer-based composite material.

[0046] In some embodiments, the core-shell particle filler and the polymer are mixed evenly by ball milling, which can make the powders more evenly mixed.

[0047] In some embodiments, after the core-shell particle filler and the polymer are uniformly mixed, the step of vacuum drying the mixture is also included.

[0048] In some embodiments, the compression molding is performed by vacuum hot pressing. In the present invention, hot pressing is performed in a vacuum environment to avoid oxidation of metal particles in the nano core-shell particles during the hot pressing process.

[0049] The core-shell particle filler (shell is graphene, center core is nano metal particle) in the present invention can be used as solid lubricant, on the one hand, the filler has self-reinforcement as nanoparticle, wherein graphene has high modulus and high strength single-layer structure, low shear force between adjacent atomic layers makes it easy for atomic layers to slide, and it has high specific surface area, it is easy to adsorb on the contact surface, thereby preventing direct contact of friction pairs; in the friction process, the outer layer of flaky graphene is peeled off from the surface of the core-shell particle, and forms a transfer film together with the peeled polymer matrix, and the inner core metal nanoparticles are exposed, the metal nanoparticles have an ideal spherical shape and good dispersibility, and the metal nanoparticles can act as "nano bearings" in the friction process, converting sliding friction into rolling friction, thereby reducing the friction coefficient and showing excellent anti-friction performance. On the other hand, the filler can well improve the friction performance of the composite material at a lower content, has good wear resistance and self-lubricating property, can effectively solve the dispersion problem of the filler in the matrix, and reduce costs.

[0050] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the examples, but the content of the present invention is not limited to the following examples. The raw materials and reagents used in the examples can be obtained through commercial channels unless otherwise specified.

[0051] The polymer used in the embodiment is one of polyetheretherketone (PEEK), polyphenylene sulfide (PPS), polyetherimide (PEI), and nylon (PA), and all are fine powders with a particle size of less than 100 μm; the polymer models used are PEEK (150PF), PPS (DIC FZ1160), PEI (Ultem 1000), and PA66 (Zytel 101LNC010). The fillers used in the comparative example are graphite (Graphite, 8000 mesh), polytetrafluoroethylene (PTFE, D50 = 10 μm), short carbon fiber (SCF, diameter 5-10 μm, aspect ratio 5: 1-10: 1), and spherical copper powder (Cu, diameter 1 μm).

[0052] The diameter of the core-shell particles prepared in the examples is 100nm-300nm.

[0053] The β-diketone metal complex used in the examples is wherein R1 and R2 are each independently selected from CH3-, C2H5-, n-C3H7-, i-CH3, n-C4H9-, i-C4H9-, s-C4H9-, t-C4H9-, CH3O-, C2H5O-, Ph-, p-CH3-Ph-, p-C2H5-Ph-, p-CH3O-Ph- or p-C2H5O-Ph-, and M n+ Cu 2+ 、Ag +、Zn 2+ Sn 2+ or Al 3+ .

[0054] Example 1

[0055] Under 60Pa vacuum conditions, 10g of β-diketone metal complex (wherein R1=R2=CH3-, M n+ Cu 2+ ) was heated to 550°C in a tube furnace, H2 (under argon protection) was introduced to reduce the β-diketone metal complex, and the temperature was kept for 180 minutes. After natural cooling, the unreacted β-diketone metal complex in the product was washed with ethanol, then centrifuged, and then dried in a vacuum oven at 60°C for 14 hours. The SEM image of the obtained Cu@Gr core-shell particles is attached. Figure 1 It can be seen that the Cu@Gr core-shell particles present a good spherical core-shell structure, graphene can be evenly coated on the surface of nanometal particles, and the particle size of the Cu@Gr core-shell particles is mostly in the range of 100nm-300nm, indicating that this method can prepare Cu@Gr core-shell particles with uniform particle size distribution and complete core-shell structure.

[0056] 0.5g, 1.5g, 2.5g, 5g Cu@Gr core-shell particles and 20g PEEK were placed in a planetary ball mill and mixed at 0°C and 200rpm for 8 hours. After mixing, the composite powder was placed in a vacuum drying oven at 100°C and dried for 2 hours.

[0057] The composite materials obtained by molding the above four dried composite materials under 10 MPa and 360°C were respectively named 0.5g-Cu@Gr-PEEK, 1.5g-Cu@Gr-PEEK, 2.5g-Cu@Gr-PEEK and 5g-Cu@Gr-PEEK.

[0058] Example 2

[0059] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = C2H5-, R2 = C3H7-, M n+ Ag + ), Cu@Gr core-shell particles were changed to Ag@Gr core-shell particles, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Ag@Gr-PEEK, 1.5g-Ag@Gr-PEEK, 2.5g-Ag@Gr-PEEK, and 5g-Ag@Gr-PEEK.

[0060] Example 3

[0061] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = Ph-, R2 = CH3-, M n+ Sn 2+ ), H2 reduction of β-diketone metal complex was changed to CO reduction, Cu@Gr core-shell particles were changed to Sn@Gr core-shell particles, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Sn@Gr-PEEK, 1.5g-Sn@Gr-PEEK, 2.5g-Sn@Gr-PEEK, and 5g-Sn@Gr-PEEK.

[0062] Example 4

[0063] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = Ph-, R2 = CH3O-, M n+ Cu 2+ ), PEEK was changed to PPS, the hot pressing temperature of 360°C was changed to 320°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Cu@Gr-PPS, 1.5g-Cu@Gr-PPS, 2.5g-Cu@Gr-PPS, and 5g-Cu@Gr-PPS, respectively.

[0064] Example 5

[0065] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = C3H7-, R2 = CH3O-, M n+ For Al 3+ ), Cu@Gr core-shell particles were changed to Al@Gr core-shell particles, PEEK was changed to PPS, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 320°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Al@Gr-PPS, 1.5g-Al@Gr-PPS, 2.5g-Al@Gr-PPS, and 5g-Al@Gr-PPS, respectively.

[0066] Example 6

[0067] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = C4H9-, R2 = C2H5O-, M n+ Zn 2+ ), Cu@Gr core-shell particles were changed to Zn@Gr core-shell particles, PEEK was changed to PPS, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 320°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Zn@Gr-PPS, 1.5g-Zn@Gr-PPS, 2.5g-Zn@Gr-PPS, and 5g-Zn@Gr-PPS, respectively.

[0068] Example 7

[0069] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = p-CH3-Ph-, R2 = CH3-, M n+ Zn 2+ ), H2 reduction of β-diketone metal complex was changed to CO reduction, Cu@Gr core-shell particles were changed to Zn@Gr core-shell particles, PEEK was changed to PEI, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 340°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Zn@Gr-PEI, 1.5g-Zn@Gr-PEI, 2.5g-Zn@Gr-PEI, and 5g-Zn@Gr-PEI, respectively.

[0070] Example 8

[0071] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = p-CH3O-Ph-, R2 = Ph-, M n+ Ag + ), Cu@Gr core-shell particles were changed to Ag@Gr core-shell particles, PEEK was changed to PEI, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 340°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Ag@Gr-PEI, 1.5g-Ag@Gr-PEI, 2.5g-Ag@Gr-PEI, and 5g-Ag@Gr-PEI, respectively.

[0072] Example 9

[0073] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1 = i-C4H9-, R2 = C2H5O-, M n+ Sn 2+ ), Cu@Gr core-shell particles were changed to Sn@Gr core-shell particles, PEEK was changed to PEI, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 340°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Sn@Gr-PEI, 1.5g-Sn@Gr-PEI, 2.5g-Sn@Gr-PEI, and 5g-Sn@Gr-PEI, respectively.

[0074] Example 10

[0075] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1=R2=Ph-, M n+ Cu 2 +), H2 reduction of β-diketone metal complex was changed to CO reduction, PEEK was changed to PA66, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 280°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Cu@Gr-PA66, 1.5g-Cu@Gr-PA66, 2.5g-Cu@Gr-PA66, and 5g-Cu@Gr-PA66, respectively.

[0076] Embodiment 11

[0077] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1=R2=CH3-, M n+ Ag + ), Cu@Gr core-shell particles were changed to Ag@Gr core-shell particles, PEEK was changed to PA66, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 280°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Ag@Gr-PA66, 1.5g-Ag@Gr-PA66, 2.5g-Ag@Gr-PA66, and 5g-Ag@Gr-PA66, respectively.

[0078] Example 12

[0079] The method is the same as in Example 1, except that the β-diketone metal complex (wherein R1=R2=CH3-, M n+ For Al 3 + ), Cu@Gr core-shell particles were changed to Al@Gr core-shell particles, PEEK was changed to PA66, and the hot pressing temperature of 360°C was changed to the hot pressing temperature of 280°C, and other conditions remained unchanged. The obtained composite materials were recorded as 0.5g-Al@Gr-PA66, 1.5g-Al@Gr-PA66, 2.5g-Al@Gr-PA66, and 5g-Al@Gr-PA66, respectively.

[0080] Comparative Example 1

[0081] Take 20g PEEK, 20g PPS, 20g PEI, and 20g PA66 and place them in a vacuum drying oven at 100°C for 2 hours. After drying, place them in a mold and cold press them at 40MPa for 10 minutes. Then place the mold in a vacuum hot press, set the temperatures to 360°C, 320°C, 340°C, and 280°C, set the pressure to 10MPa, and hot press them for 80 minutes. After the mold cools down naturally, take out the comparison samples, and the comparison samples are recorded as PEEK, PPS, PEI, and PA66.

[0082] Comparative Example 2

[0083] 2g, 5g, 10g, 15g of Graphite and 20g of PEEK were placed in a planetary ball mill and mixed at 0°C and 200rpm for 8 hours. After mixing, the composite material powder was placed in a vacuum drying oven at 100°C and dried for 2 hours.

[0084] The composite materials obtained by molding the above four dried composite materials under the conditions of 10 MPa and 360° C. were respectively recorded as 2g-Graphite / PEEK, 5g-Graphite / PEEK, 10g-Graphite / PEEK, and 15g-Graphite / PEEK.

[0085] Comparative Example 3

[0086] The method is the same as that of Comparative Example 2, except that Graphite is changed to PTFE, PEEK is changed to PPS, and the hot pressing temperature of 360°C is changed to 320°C, and other conditions remain unchanged. The obtained composite materials are respectively recorded as 2g-PTFE / PPS, 5g-PTFE / PPS, 10g-PTFE / PPS, and 15g-PTFE / PPS.

[0087] Comparative Example 4

[0088] The method is the same as that of Comparative Example 2, except that Graphite is adjusted to a mixture of PTFE and SCF (the mass ratio of PTFE to SCF is 1:1), PEEK is adjusted to PEI, and the hot pressing temperature of 360°C is adjusted to a hot pressing temperature of 340°C, and other conditions remain unchanged. The obtained composite materials are recorded as 2g-PTFE / SCF / PEI, 5g-PTFE / SCF / PEI, 10g-PTFE / SCF / PEI, and 15g-PTFE / SCF / PEI.

[0089] Comparative Example 5

[0090] The method is the same as that of Comparative Example 2, except that Graphite is adjusted to a mixture of Graphite and Cu (the mass ratio of Graphite to Cu is 1:1), PEEK is adjusted to PA66, and the hot pressing temperature of 360°C is adjusted to the hot pressing temperature of 280°C, and other conditions remain unchanged. The obtained composite materials are respectively recorded as 2g-Graphite / Cu / PA66, 5g-Graphite / Cu / PA66, 10g-Graphite / Cu / PA66, and 15g-Graphite / Cu / PA66.

[0091] Performance Testing

[0092] The composite materials prepared in Examples 1-12 and the comparative samples prepared in Comparative Examples 1-5 were subjected to friction loss performance tests. The plate samples after vacuum hot pressing were processed into 2.5×2.5×20 mm 3 The rectangular splines are used for friction testing, and the tribological performance tests are carried out using a friction loss testing machine.

[0093] The test model adopts a pin-ring model, in which the pin is a composite material, the ring is GCr steel, the roughness of the ring is 0.15-0.2, the diameter of the ring is 48mm, and the test conditions are 1MPa, 200rpm, 3h. The results are shown in Table 1-4.

[0094] Table 1: Friction coefficient and specific wear rate of PEEK, Cu@Gr-PEEK, Ag@Gr-PEEK, Sn@Gr-PEEK, and Graphite / PEEK

[0095]

[0096] Table 2: Friction coefficient and specific wear rate of PPS, Cu@Gr-PPS, Al@Gr-PPS, Zn@Gr-PPS, and PTFE / PPS

[0097]

[0098]

[0099] Table 3: Friction coefficient and specific wear rate of PEI, Zn@Gr-PEI, Ag@Gr-PEI, Sn@Gr-PEI, and PTFE / SCF / PEI

[0100]

[0101]

[0102] Table 4: Friction coefficient and specific wear rate of PA66, Cu@Gr-PA66, Ag@Gr-PA66, Al@Gr-PA66, Graphite / Cu / PA66

[0103]

[0104]

[0105] It can be seen from Tables 1 to 4 that, compared with pure polymers (PEEK, PPS, PEI, PA66), polymers with a single filler can often only improve partial friction properties, and the remaining friction properties may decrease with the addition of fillers; adding multiple fillers often requires the filler content to reach more than 30% to achieve the best effect, and the negative impact caused by the increase in filler content limits the improvement in friction properties; the polymer-based composite material filled with nano core-shell particles of the present invention has a low friction coefficient and specific wear rate, indicating that the core-shell particles can effectively enhance the tribological properties of the polymer, and when the content of the core-shell particles in the composite material is about 7.5%, the composite material has the best friction and wear properties, and the low content of the filler material can effectively solve the problem of poor dispersion of the filler in the matrix, and better improve the tribological properties of the polymer.

[0106] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A core-shell particle filler, characterized in that: The shell is graphene, and the central core is a nano metal particle; the diameter of the core-shell particle filler is 100nm-300nm.

2. The core-shell particle filler according to claim 1, characterized in that The nano metal particles include Cu, Ag, Zn, Sn or Al.

3. A method for preparing the core-shell particle filler according to claim 1 or 2, characterized in that: Under vacuum conditions, the β-diketone metal complex is heated, and then a reducing gas is introduced to keep the temperature to reduce the β-diketone metal complex, thereby obtaining the core-shell particle filler; The structural formula of the β-diketone metal complex is: wherein R1 and R2 are each independently selected from CH3-, C2H5-, n-C3H7-, i-CH3, n-C4H9-, i-C4H9-, s-C4H9-, t-C4H9-, CH3O-, C2H5O-, Ph-, p-CH3-Ph-, p-C2H5-Ph-, p-CH3O-Ph- or p-C2H5O-Ph-; M n+ Cu 2+ 、Ag + 、Zn 2+ Sn 2+ or Al 3+ .

4. The method for preparing the core-shell particle filler according to claim 3, characterized in that: The vacuum condition is a vacuum degree ≤ 60Pa.

5. The method for preparing the core-shell particle filler according to claim 3, characterized in that: The temperature for heating the β-diketone metal complex is 450-600° C.; and the insulation time is 150-200 minutes.

6. The method for preparing the core-shell particle filler according to claim 3, characterized in that: The reducing gas includes CO or H2.

7. Use of the core-shell particle filler according to claim 1 or 2 in the preparation of polymer-based composite materials.

8. A polymer-based wear-resistant composite material filled with core-shell particles, characterized in that: The raw materials include a polymer and the core-shell particle filler according to claim 1 or 2.

9. The core-shell particle filled polymer-based wear-resistant composite material according to claim 8, characterized in that: The polymer is polyetheretherketone, polyphenylene sulfide, polyimide, polyetherimide, nylon 66 or polyoxymethylene.

10. A method for preparing the core-shell particle filled polymer-based wear-resistant composite material according to claim 8, characterized in that: The core-shell particle filler according to claim 1 or 2 is mixed evenly with a polymer, and then molded to obtain the polymer-based composite material filled with the core-shell particles.

Citation Information

Patent Citations

  • Metal / graphene composite material and preparation method thereof

    CN105215353A

  • A composite material, a molded product including the same and a method of preparing a polymer filament

    CN106674931A

  • Molybdenum disulfide quantum dot / graphene / polymer-based super-wear-resistant self-lubricating composite material and preparation method and application thereof

    CN111662547A

  • Two-dimensional graphene-coated copper composite material with core-shell structure and preparation method and application thereof

    CN111757657A