Modified maleimide prepolymer, resin composition and application thereof
Modification of maleimide resin and resin composition with a pterene-containing aromatic amine compound, the deformation problem of circuit board in high temperature process is solved, the heat resistance and dielectric properties are improved, and the high functionalization is met Requirements for circuit boards.
Patent Information
- Application Number
- CN202411321344.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
The existing bismaleimide resins are prone to deformation during high-temperature processes, resulting in abnormal signal transmission, and have problems such as high curing temperature, large water absorption, and high brittleness, making it difficult to meet the needs of highly functional circuit boards.
The maleimide resin is modified with an aromatic amine compound containing a pterene structure, and the modified maleimide prepolymer is formed by prepolymerization reaction, and the cyanate compound, epoxy resin and inorganic filler are combined to form a Resin composition to improve glass transition temperature, heat resistance and dielectric properties.
It has obtained cured substances with high heat resistance, high toughness, low CTE, low dielectricity and low water absorption, which has improved the overall performance of the circuit board and is suitable for electronic equipment with multilayer, high wiring density and high signal speed .
Smart Images

Figure BDA0005054014310000021 
Figure BDA0005054014310000031 
Figure BDA0005054014310000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminates, and in particular to a modified maleimide prepolymer, a resin composition and applications thereof. Background Art
[0002] In recent years, as electronic signal transmission methods develop towards 5G, and electronic equipment, communication devices, personal computers, etc. are becoming more functional and miniaturized, the circuit boards used are also developing towards multi-layering, high-density wiring, and high-speed signal transmission, which puts higher requirements on the comprehensive performance of circuit substrates such as copper clad laminates. In order to avoid deformation of copper clad laminates caused by the use of high-temperature processes during product processing, which in turn causes defects in subsequent products and causes abnormal signal transmission, it is necessary to develop copper clad laminate materials with a lower thermal expansion coefficient.
[0003] Bismaleimide resin has excellent heat resistance, high modulus, low CTE, and is therefore widely used in high performance printed circuit boards. However, there are problems such as high curing temperature, large water absorption, large brittleness in bismaleimide resin. In order to improve the above-mentioned shortcomings of maleimide resin, diamine or allyl compound modification is generally used at present, wherein, the product after modified bismaleimide with aromatic diamine compounds is all improved to a certain extent in solubility and toughness, but the aromatic diamine toxicity is larger, and the modified product can only be dissolved in high boiling point polar solvents (such as DMF, NMP etc.), and it still has a large improvement space in toughness, heat resistance, dielectricity and water absorption. For example, the prior art JP2004359599A discloses a method for producing triptylenediamine, a method for preparing triptylenediamine, which comprises nitrating a triptylenediamine derivative and then reducing the obtained nitro-substituted triptylenediamine; the prior art CN108291028 discloses ortho-substituted triptylenediamines, monomers and polymers based on triptylenes, preparation methods and uses thereof, including 3,6-dimethyl-2,7-diaminotriptylenediamine derivatives.
[0004] Therefore, the present invention provides a modified maleimide prepolymer, a resin composition and applications thereof to obtain a cured product with high heat resistance, high toughness, low CTE, low dielectric properties and low water absorption, thereby obtaining a cured product with excellent comprehensive performance. Summary of the invention
[0005] The object of the present invention is to provide a modified maleimide prepolymer, a resin composition and applications thereof, so as to obtain a cured product with high heat resistance, high toughness, low CTE, low dielectric properties and low water absorption, thereby obtaining a cured product with excellent comprehensive performance.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A modified maleimide prepolymer is prepared by prepolymerizing 100 parts of a maleimide resin and 1 to 100 parts of a pterylene-containing modifier, wherein the pterylene-containing modifier is represented by the structural formula (1) or / and the structural formula (2):
[0008]
[0009] Wherein, R1, R2 and R3 are the same or different and are hydrogen, C1-C5 alkyl, allyl, vinyl or amino respectively, and at least one of them is amino or allyl, n is an integer of 1-5, and * is a connecting part.
[0010] Preferably, at least two of R1, R2 and R3 in the structural formula (1) and the structural formula (2) are amino groups.
[0011] Preferably, the compound with n=1 in the pterene-containing modifier contains 50 to 100 parts.
[0012] Preferably, the prepolymerization reaction temperature is 60 to 220° C., and the reaction time is 0.5 to 8 hours.
[0013] More preferably, the prepolymerization reaction temperature is 110-150° C., and the reaction time is 1 hour, 2 hours, 3 hours, 4 hours or 5 hours.
[0014] Preferably, the 1 to 100 parts of the pterene-containing modifier are aromatic amine compounds.
[0015] Preferably, the method of the prepolymerization reaction is not particularly limited. The aromatic amine compound and the maleimide resin are dissolved and dispersed in an appropriate amount of an organic solvent, heated to 60 to 180° C. under nitrogen protection and kept reacting under stirring conditions for 0.5 to 5 hours to obtain an amine-modified bismaleimide prepolymer.
[0016] Preferably, the organic solvent is selected from at least one of acetone, butanone, toluene, methyl isobutyl ketone, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0017] Further preferably, an auxiliary agent is added during the prepolymerization of the maleimide resin and the modifier to control the overall reaction rate, improve the processability, and improve the comprehensive properties of the cured product.
[0018] Preferably, 100 parts of maleimide resin, 1 to 100 parts of a pteryl-containing modifier and 0.5 to 5 parts of an auxiliary agent are reacted to generate the modified maleimide prepolymer.
[0019] Preferably, the auxiliary agent is selected from at least one of aminophenol, carboxylic acid or carboxylic anhydride.
[0020] Preferably, the method of the prepolymerization reaction is not particularly limited. The modifier, maleimide resin and auxiliary agent are dissolved and dispersed in an appropriate amount of organic solvent, heated to 60-180° C. under nitrogen protection and kept reacting for 0.5-5 hours under stirring conditions to obtain a modified bismaleimide prepolymer.
[0021] Preferably, the modified maleimide prepolymer further comprises unmodified maleimide resin.
[0022] In the above technical solution, the maleimide resin is at least one selected from the following structures:
[0023]
[0024] R2 is hydrogen, methyl or ethyl, R1 is methylene, ethylene or, n is an integer from 1 to 10;
[0025]
[0026] n is an integer from 1 to 10;
[0027] n is an integer from 1 to 10;
[0028] n is an integer from 1 to 10;
[0029]
[0030] R is hydrogen, methyl or ethyl, and n is an integer from 1 to 10;
[0031] R is a methyl group, and n is an integer of 1-20.
[0032] For further example, the maleimide resin is selected from BMI-1000, BMI-2300, BMI-5100 or BMI-TMH manufactured by Yamato Chemical; BMI, BMI-70 or BMI-80 manufactured by KI Chemical; X9-470, X9-450 or X-9500 manufactured by DIC; MIR-3000 or MIR-5000 manufactured by Nippon Kayaku.
[0033] The present application also claims protection for a resin composition, wherein the resin composition contains the modified maleimide prepolymer.
[0034] Preferably, the resin composition includes a cyanate compound.
[0035] Preferably, the resin composition comprises, by weight:
[0036] Modified maleimide prepolymer: 10-80 parts;
[0037] Cyanate compound: 5 to 60 parts.
[0038] In the above technical scheme, the cyanate ester compound is selected from at least one of bisphenol A type cyanate ester compounds, bisphenol F type cyanate ester compounds, bisphenol E type cyanate ester compounds, bisphenol M type cyanate ester compounds, DCPD type cyanate ester compounds, naphthalene type cyanate ester compounds, biphenyl type cyanate ester compounds, and triphenyl type cyanate ester compounds.
[0039] The cyanate compound is a monomer, a prepolymer or a mixture thereof.
[0040] Preferably, the resin composition further comprises epoxy resin and / or polyphenylene ether resin.
[0041] Preferably, the epoxy resin is selected from any one or a combination of at least two of dicyclopentadiene epoxy resin, epoxy resin containing unsaturated carbon-carbon double bonds, phosphorus-containing epoxy resin, isocyanate-modified epoxy resin, biphenyl epoxy resin, bisphenol A epoxy resin, phenol novolac epoxy resin, o-cresol novolac epoxy resin, epoxidized polybutadiene resin, epoxy resin containing naphthalene rings, bisphenol F epoxy resin, trifunctional epoxy resin, hydrogenated bisphenol A epoxy resin or hydrogenated bisphenol F epoxy, and its content is 5 to 60 parts.
[0042] More preferably, the molecular terminal of the polyphenylene ether in the polyphenylene ether resin contains an unsaturated double bond, and OPE-2St series manufactured by Mitsubishi Gas or SA9000 manufactured by Sabic are preferably used.
[0043] Preferably, the content of the polyphenylene ether resin is 20 to 90 parts.
[0044] In the above technical solution, the resin composition also includes 30 to 200 parts of inorganic filler.
[0045] Preferably, the inorganic filler is selected from one or a combination of any of non-metallic oxides, metal nitrides, non-metallic nitrides, inorganic hydrates, inorganic salts, metal hydrates or inorganic phosphorus.
[0046] More preferably, the inorganic filler is selected from at least one of fused silica, crystalline silica, spherical silica, hollow silica, aluminum hydroxide, aluminum oxide, talc, aluminum nitride, boron nitride, silicon carbide, barium sulfate, barium titanate, strontium titanate, calcium carbonate, calcium silicate, mica, and glass fiber powder.
[0047] More preferably, the inorganic filler is silicon dioxide.
[0048] More preferably, the inorganic filler is spherical silica treated with a surface treatment agent.
[0049] Preferably, the surface treatment agent is a silane coupling agent, such as a silane coupling agent containing an epoxy group, an amino group, a vinyl group, an acrylate group or an allyl group.
[0050] Preferably, the median particle size of the inorganic filler is 1 to 15 microns, for example, 1 micron, 2 microns, 5 microns, 8 microns, 10 microns, 11 microns, 12 microns, 13 microns, 14 microns.
[0051] More preferably, the median particle size of the inorganic filler is 1 to 10 microns.
[0052] In the above technical solution, the resin composition also includes a catalyst, and its content is 0.01 to 8 parts.
[0053] Preferably, the catalyst is selected from at least one of imidazoles, pyridines, organophosphorus or metal salts.
[0054] Preferably, the imidazole is selected from at least one of 4-dimethylaminopyridine, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, modified imidazole and zinc octanoate.
[0055] In the above technical solution, the resin composition also includes a flame retardant, which contains 5 to 60 parts.
[0056] Preferably, the flame retardant is selected from at least one of a bromine flame retardant, a phosphorus flame retardant, a nitrogen flame retardant, an organosilicon flame retardant, and an organometallic salt flame retardant.
[0057] Preferably, the brominated flame retardant is selected from at least one of decabromodiphenyl ether, decabromodiphenyl ethane, brominated styrene or tetrabromophthalamide.
[0058] Preferably, the phosphorus flame retardant is selected from inorganic phosphorus, condensed phosphate, phosphoric acid, hypophosphite, phosphorus oxide, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO-HQ), (m is an integer from 1 to 5), At least one of 10-phenyl-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, tri(2,6-dimethylphenyl)phosphine, phosphazene, and modified phosphazene; wherein the DOPO group in the above structure is
[0059] Preferably, the flame retardant is a condensed phosphate ester, a hypophosphite or a bis-DOPO compound.
[0060] The present application also claims protection for the use of the resin composition in prepregs, laminates, insulating films, insulating boards, copper-clad boards, circuit substrates and electronic devices.
[0061] Specifically, the prepreg comprises a reinforcing material and the above-mentioned resin composition attached to the surface of the reinforcing material.
[0062] Preferably, the preparation method of the prepreg is:
[0063] Dissolving the resin composition with a solvent to prepare a resin composition glue solution;
[0064] The reinforcing material is immersed in the resin composition glue solution, and the immersed reinforcing material is taken out and baked at a temperature of 100 to 180° C. for 1 to 15 minutes, and the semi-cured sheet can be obtained after drying.
[0065] Preferably, the solvent is selected from at least one of acetone, butanone, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0066] Preferably, the reinforcing material is selected from at least one of natural fibers, organic synthetic fibers, organic fabrics, and inorganic fabrics. Preferably, the reinforcing material is glass fiber cloth, and the glass fiber cloth is preferably open fiber cloth or flat cloth. More preferably, the glass fiber cloth is E glass fiber cloth, S glass fiber cloth, T glass fiber cloth or Q glass fiber cloth.
[0067] In addition, when the reinforcing material is glass fiber cloth, the glass fiber cloth generally needs to be chemically treated to improve the bonding between the resin composition and the interface of the glass fiber cloth. The main method of the chemical treatment is coupling agent treatment. The coupling agent used is preferably an epoxy silane coupling agent or an amino silane coupling agent, so that the reinforcing material has good water resistance and heat resistance.
[0068] Preferably, the laminate comprises a piece of the above-mentioned prepreg and a metal foil arranged on at least one side of the prepreg, or the laminate comprises a composite sheet formed by overlapping a plurality of the above-mentioned prepregs and a metal foil arranged on at least one side of the composite sheet.
[0069] Preferably, the method for preparing the laminate is:
[0070] The laminated board can be obtained by coating one or both sides of the prepreg with metal foil, or by stacking at least two prepregs to form a composite sheet, coating one or both sides of the composite sheet with metal foil, and hot pressing.
[0071] The hot pressing conditions are: pressing for 2 to 4 hours at a pressure of 0.2 to 2 MPa and a temperature of 150 to 250°C.
[0072] Preferably, the metal foil is selected from copper foil or aluminum foil, and the thickness of the metal foil is not particularly limited, such as 5 μm, 8 μm, 12 μm, 18 μm, 35 μm or 70 μm.
[0073] Preferably, the insulating plate includes at least one prepreg sheet mentioned above.
[0074] Preferably, the insulating film comprises a carrier film and the above-mentioned resin composition attached to the surface of the carrier film, and the heat resistance of the insulating film is significantly improved.
[0075] Preferably, the method for preparing the insulating film is:
[0076] Dissolving the resin composition with a solvent to prepare a resin composition glue solution;
[0077] The insulating film can be obtained by coating the resin composition glue on the carrier film and heating and drying the carrier film coated with the resin composition glue.
[0078] Preferably, the solvent is selected from at least one of acetone, butanone, methyl isobutyl ketone, N,N-dimethylformamide, N,N-dimethylacetamide, ethylene glycol methyl ether, propylene glycol methyl ether, benzene, toluene, xylene and cyclohexane.
[0079] Preferably, the carrier film is selected from at least one of PET film, PP film, PE film and PVC film.
[0080] Preferably, the circuit substrate includes at least one of the prepreg and the laminate.
[0081] Preferably, the method for preparing the circuit substrate is a conventional technical means in the art and will not be described in detail here.
[0082] Preferably, the electronic device comprises the above-mentioned circuit substrate.
[0083] Preferably, the method for preparing the electronic device is a conventional technical means in the art and will not be described in detail here.
[0084] Due to the application of the above technical solution, the present invention has the following beneficial effects compared with the prior art:
[0085] 1. The present invention adopts an aromatic amine compound containing a pterygium structure to modify the maleimide resin, wherein the structure is a special spatial structure, which is composed of three benzene rings connected by a shared carbon atom. This structure makes the obtained material have high stability and reactivity, which is conducive to prepolymerization with bismaleimide to obtain a higher glass transition temperature, heat resistance, and better dielectric properties;
[0086] 2. The present invention introduces triptycene, a large rigid free volume, which can break the crystallinity of the BMI monomer, increase the distance between molecular chains, and improve the solubility of the resin prepreg in common solvents. Due to the advantages of multiple benzene rings, the disadvantage of reduced heat resistance of BMI resin due to reduced crosslinking density caused by increased diamine content is avoided. The structure increases the distance between molecular layers, generates more free space volume, makes it easier for molecular layers to slide, and thus achieves a toughening effect, thereby obtaining a cured product with high heat resistance, high toughness, low CTE, low dielectric properties, and low water absorption, thereby obtaining a cured product with relatively excellent comprehensive performance, which is conducive to its large-scale application. DETAILED DESCRIPTION
[0087] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, a specific implementation scheme is now described in detail.
[0088] The present invention is further described below in conjunction with the examples, but the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not indicated are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0089] Synthesis Example 1: Preparation of prepolymer A;
[0090] Add 40g of 100 g of maleimide resin (BMI-2300, manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were reacted at 160° C. for 100 min to obtain prepolymer A.
[0091] Synthesis Example 2: Preparation of prepolymer B;
[0092] Add 40g of 100 g of maleimide resin (BMI-2300, manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were reacted at 160° C. for 100 min to obtain prepolymer B.
[0093] Synthesis Example 3: Preparation of prepolymer C;
[0094] 100 g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were added to a beaker, and the mixture was reacted at 110°C for 60 min. After the mixture was heated to 120°C, 40 g of 4,4'-[oxybis(ethyleneoxy)]diphenylamine was added. The reaction was continued for 60 min to obtain prepolymer C.
[0095] Comparative Synthesis Example 1: Preparation of prepolymer D;
[0096] 40 g of 4,4'-diaminodiphenylmethane, 100 g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were added to a beaker and reacted at 120°C for 100 min to obtain a prepolymer D.
[0097] Comparative Synthesis Example 2: Preparation of Prepolymer E;
[0098] 40 g of 4,4'-diaminodiphenyl ether, 100 g of maleimide resin (BMI-2300 manufactured by Yamato Chemical Industry Co., Ltd.) and 2 g of p-aminophenol were added to a beaker and reacted at 120°C for 100 min to obtain a prepolymer E.
[0099] The aromatic amine compound used in Comparative Synthesis Example 2 is different from that in Synthesis Example 1. The aromatic amine compound in Comparative Synthesis Example 2 contains one ether bond.
[0100] Example 1
[0101] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer A, 30 parts of cyanate ester, 20 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0102] Example 2
[0103] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer B, 20 parts of cyanate ester, 30 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0104] Example 3
[0105] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer C, 15 parts of cyanate ester, 10 parts of epoxy resin, 125 parts of inorganic filler, and 0.5 parts of catalyst.
[0106] Example 4
[0107] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer A, 60 parts of polyphenylene ether resin, 20 parts of cross-linking agent, 180 parts of inorganic filler, and 0.5 parts of catalyst.
[0108] Comparative Example 1
[0109] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer D, 30 parts of cyanate ester, 20 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0110] Comparative Example 2
[0111] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer E, 20 parts of cyanate ester, 30 parts of epoxy resin, 150 parts of inorganic filler, and 0.5 parts of catalyst.
[0112] Comparative Example 3
[0113] This embodiment is a resin composition, which includes, by weight: 100 parts of prepolymer E, 60 parts of polyphenylene ether resin, 20 parts of cross-linking agent, 180 parts of inorganic filler, and 0.5 parts of catalyst.
[0114] The components and addition amounts of Examples 1-4 and Comparative Examples 1-3 are shown in Table 1 below.
[0115] Table 1
[0116] Components Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Prepolymer A 100 100 Prepolymer B 100 Prepolymer C 100 Prepolymer D 100 Prepolymer E 100 100 Cyanate 30 20 15 30 20 Epoxy resin 20 30 10 20 30 Polyphenylene ether resin 60 60 Crosslinking agent 20 20 Inorganic fillers 150 150 125 180 150 150 180 catalyst 0.5 0.5 0.5 0.5 0.5 0.5 0.5
[0117] The raw material manufacturers and brands of each component used in Examples 1-4 and Comparative Examples 1-3 are shown in Table 2 below.
[0118] Table 2
[0119] Components Manufacturer and brand Cyanate Made by Tianqi, bisphenol A Epoxy resin DIC, HP-6000 Polyphenylene ether resin Made by Mitsubishi, OPE-2St Crosslinking agent TAIC Inorganic fillers Silicon dioxide catalyst 2-Methylimidazole
[0120] Mixing of glue:
[0121] According to the formula in Table 1, all the components in the formula are prepared into a thermosetting resin composition glue solution with a solid content of 65%;
[0122] Then a laminate was made under the following conditions:
[0123] Reinforcement material: ordinary electronic grade 2116 glass fiber cloth;
[0124] Metal foil: 18 microns, electrolytic copper foil;
[0125] Number of layers: 6;
[0126] Thickness of sheet after forming: 0.7mm;
[0127] Pre-impregnation semi-curing conditions: 170℃ / 5min;
[0128] Curing conditions: 150℃ / 60min+220℃ / 180min.
[0129] The performance tests were carried out on the above-mentioned embodiments 1-4 and comparative examples 1-3 respectively, and the test results are shown in Table 3 below.
[0130] Table 3
[0131] Test items Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Glass transition temperature (DMA / ℃) 252 255 259 254 234 237 226 PCT water absorption (%) 0.28 0.30 0.25 0.21 0.45 0.48 0.45 CTE (X / Y axis) (ppm / ℃) 7.1 6.6 7.4 7.5 11.0 9.9 11.1 Peel strength (N / mm) 1.0 0.97 1.12 0.88 1.1 0.96 0.89 Dielectric constant (10GHz) 3.4 3.41 3.47 3.12 3.79 3.67 3.51 Dielectric loss (10GHz) 0.004 0.004 0.004 0.0028 0.0071 0.0065 0.0050 Elastic modulus(GPa) 28 28 31 33 23 25 24
[0132] The performance of the above-mentioned Examples 1-4 and Comparative Examples 1-3 was tested as follows:
[0133] (1) Glass transition temperature (Tg): dynamic mechanical properties tester (TADMAQ800, USA) was used with a heating rate of 10 °C / min and a nitrogen atmosphere;
[0134] (2) Dk and Df: measured at 10 GHz using the flat plate method in accordance with IPC-TM-6502.5.5.9;
[0135] (3) CTE (X / Y) determination: TMA (thermomechanical analysis) was used, with a heating rate of 10°C / min and a test temperature range of 30 to 100°C;
[0136] (4) PCT water absorption rate: Take 3 samples of 10 cm × 10 cm, 0.80 mm thick, with metal foil removed from both sides, dry them at 120°C for 2 hours, weigh them, and record the weight as W1. Then use a pressure cooker tester to treat them at 121°C and 2 atmospheres for 12 hours. After absorbing the free water on the surface, put them in a desiccator and cool them down. Then weigh them as W2. The water absorption rate of the board is calculated based on the weight before and after.
[0137] (5) Peel strength (PS): The peel strength of the metal cover layer was tested using a laminate according to the “after thermal stress” test conditions in the IPC-TM-650 method.
[0138] (6) Elastic modulus: measured according to the DMA method specified in IPC-TM-6502.4.24.4;
[0139] (7) Appearance quality: Visually inspect the appearance of the CCL substrate. A substrate without obvious glue deficiency or pinholes has a good appearance. A substrate with glue deficiency or pinholes has a fair appearance.
[0140] In summary, the present invention uses an aromatic amine compound containing a cyclopentene structure to modify the maleimide resin, wherein the structure is a special spatial structure form, which is composed of three benzene rings connected by a common carbon atom. This structure makes the obtained material have high stability and reactivity, which is conducive to prepolymerization with bismaleimide to obtain a higher glass transition temperature, heat resistance, and more excellent dielectric properties; the present invention introduces a large rigid free volume of triptycene, which can break the crystallinity of the BMI monomer, increase the distance between molecular chains, and improve the solubility of the resin prepreg in common solvents. Due to the advantages of multiple benzene rings, the disadvantage of reducing the heat resistance of the BMI resin due to the increase in diamine content and the reduction in crosslinking density is avoided. The structure increases the distance between molecular layers and generates more free space volume, making it easier for molecular layers to slide between layers, thereby achieving a toughening effect, and obtaining a cured product with high heat resistance, high toughness, low CTE, low dielectric properties, and low water absorption, thereby obtaining a cured product with relatively excellent comprehensive performance, which is conducive to its large-scale application.
[0141] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A modified maleimide prepolymer, characterized in that: By weight, 100 parts of maleimide resin and 1 to 100 parts of a pterygium-containing modifier are prepolymerized to form a pterygium-containing modifier, wherein the pterygium-containing modifier is represented by the structural formula (1) or / and the structural formula (2): Wherein, R1, R2 and R3 are the same or different and are hydrogen, C1-C5 alkyl, allyl, vinyl or amino respectively, and at least one of them is amino or allyl, n is an integer of 1-5, and * is a connecting part.
2. The modified maleimide prepolymer according to claim 1, characterized in that In the structural formula (1) and the structural formula (2), at least two of R1, R2 and R3 are amino groups.
3. The modified maleimide prepolymer according to claim 1, characterized in that: The compound with n=1 in the pterene-containing modifier contains 50 to 100 parts.
4. The modified maleimide prepolymer according to claim 1, characterized in that: 100 parts of maleimide resin, 1 to 100 parts of a pterene-containing modifier and 0.5 to 5 parts of an auxiliary agent are reacted to generate the modified maleimide prepolymer.
5. The modified maleimide prepolymer according to claim 4, characterized in that: The auxiliary agent is selected from at least one of aminophenol, carboxylic acid or carboxylic anhydride.
6. The modified maleimide prepolymer according to claim 1, characterized in that: The modified maleimide prepolymer also includes unmodified maleimide resin.
7. A resin composition, characterized in that The resin composition contains the modified maleimide prepolymer according to any one of claims 1 to 6.
8. The resin composition according to claim 7, characterized in that The resin composition includes a cyanate compound.
9. The resin composition according to claim 7 or 8, characterized in that By weight, including: Modified maleimide prepolymer: 10-80 parts; Cyanate compound: 5 to 60 parts.
10. Use of the resin composition according to any one of claims 7 to 9 in prepregs, laminates, insulating films, insulating boards, copper-clad boards, circuit substrates and electronic devices.
Citation Information
Cited By
Modified maleimide prepolymer and resin composition
CN121248933A
Modified maleimide prepolymers and resin compositions
CN121248933B