A kind of aviation cable coating material and preparation method thereof
By combining modified concave and concave rock stone and thermal filler, the flame retardant and thermal conductivity of aviation cable clad materials are improved, and the flame retardant performance of existing materials is solved, which significantly improves the breaking strength of the material and the service life of the cable.
Patent Information
- Application Number
- CN202411268943.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The flame retardant performance of existing aviation cable coating materials is insufficient, making it difficult to effectively inhibit the release of smoke and oxygen inflow, resulting in incomplete combustion and affecting the safety performance of the cable.
By modifying the concave and convex rod stones, combined with titanate coupling agent, a modified concave and convex rod is formed; hexagonal boron nitride and spherical alumina are pretreated to prepare thermal fillers, and chlorinated regenerated rubber is added to the material. , a solid coking layer is formed to improve flame retardancy.
The modified concave and concave rock stone provides hard units in the material to improve fracture strength and flame retardant performance; thermal fillers build thermal conductivity channels, reduce cable temperature and improve service life; chlorinated regenerated rubber forms a coking layer to prevent continued combustion, significantly Improve flame retardant and aging resistance.
Smart Images

Figure CN118772517B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cable coating materials, in particular to an aviation cable coating material and a preparation method thereof. Background Art
[0002] The main function of aviation cable covering materials is to protect cables, extend cable life, reduce mechanical losses, and provide safety performance such as fire prevention and heat insulation.
[0003] The Chinese patent with publication number CN110330736A discloses a cable insulation coating material, which is made of the following components in parts by weight: 20-30 parts of polyvinyl chloride, 3-5 parts of ceramic micropowder, 15-25 parts of modified alkyd resin, 10-20 parts of phenolic resin, 5-30 parts of potassium humate, 4-6 parts of polyethylene wax, 2-5 parts of cellulose acetate, 1-2 parts of zinc borate, 1-2 parts of coupling agent, 3-5 parts of epoxy soybean oil, 4-10 parts of modified rosin rock, and 5-10 parts of anti-aging agent. Preferably, it also includes 5-10 parts of xylene and 20-30 parts of polycarbonate. Preferably, the anti-aging agent is made of the following components in parts by weight: 350-400 parts of acrylic resin aqueous solution, 200-250 parts of zeolite powder suspension, 3-5 parts of maleic anhydride, and 5-10 parts of polypropylene glycol. Preferably, the coupling agent is titanate, aluminate, zirconate or borate. Preferably, the mass ratio of cellulose acetate to zinc borate is 1:1. The invention has reasonable raw material selection, safe use, good aging resistance, solves the problem of easy aging of the cable coating, can extend the service life, has good insulation performance, and has excellent thermal stability. However, the flame retardant performance of the cable coating material prepared by the above-mentioned prior art needs to be improved; for this reason, the present invention provides an aviation cable coating material and a preparation method thereof to solve the above-mentioned problems. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides an aviation cable coating material and a preparation method thereof, which solves the problems mentioned in the above background technology.
[0005] To achieve the above purpose, the present invention is implemented by the following technical scheme: an aviation cable coating material, the aviation cable coating material comprises the following components in parts by weight: 100-120 parts of polyethylene resin, 35-45 parts of chlorinated regenerated rubber, 0.8-2 parts of flame retardant, 1.5-2.5 parts of thermal conductive filler, 1-4 parts of antioxidant, and 2-6 parts of plasticizer;
[0006] The flame retardant is modified attapulgite, and the specific modification method is:
[0007] (1) Grind the attapulgite into powder and dry it in a drying oven at 70 to 80°C for 10 to 12 hours;
[0008] (2) Take out the obtained product, add a titanate coupling agent thereto at room temperature, stir and mix, and thus obtain a modified attapulgite.
[0009] Preferably, the mass ratio of the attapulgite to the titanate coupling agent is (97-99):1, and the titanate coupling agent is TM931.
[0010] Preferably, in said (2), the specific stirring method is: first stirring at a speed of 300-500 r / min for 5-8 min, and after a mixture of agglomerated particles and powder exists, stirring at a high speed of 20000-25000 r / min for 2-3 min, and then standing for 1-2 min, and repeating the operation 3 times.
[0011] Preferably, the preparation method of the thermally conductive filler is:
[0012] Ⅰ. Alkali treatment of hexagonal boron nitride;
[0013] Ⅱ. Pre-treating the surface of spherical alumina;
[0014] III. Place the treated hexagonal boron nitride and spherical alumina in ethanol at a mass ratio of 1:(2.5-3) and perform ultrasonic treatment for 30-40 minutes;
[0015] IV. Stir and mix the two solutions to obtain a thermally conductive filler.
[0016] Preferably, in said Ⅰ, the specific alkali treatment method of hexagonal boron nitride is: add 280-300mL of 5mol / L sodium hydroxide solution to 10-12g of hexagonal boron nitride, heat to boiling after mixing, reflux and stir, wash with distilled water until neutral, and then place in a vacuum drying oven at 85-90°C for drying.
[0017] Preferably, in said III, the specific method for pretreating the surface of spherical alumina is: mixing KH550 with distilled water to obtain a mixed solution 1; mixing KH550 with anhydrous ethanol to obtain a mixed solution 2; mixing the mixed solution 1 with the mixed solution 2, and heating the mixture to 30-35°C in a water bath, reacting for 30-40 minutes to obtain a hydrolyzate; dividing the hydrolyzate into three portions, pouring them into a mixer containing spherical alumina in sequence, heating to 105-115°C and stirring.
[0018] Preferably, the molar ratio of KH550 to distilled water is 1:(2.6-3), and the volume ratio of KH550 to anhydrous ethanol is 1:(0.9-1).
[0019] Preferably, the preparation method of the chlorinated regenerated rubber is as follows: pour 500 mL of distilled water into 90 to 100 g of regenerated rubber particles, heat to 70 to 80° C. and stir, then add 0.6 to 0.9 g of azobisisobutyronitrile, and pass Cl2 until the chlorine content reaches equilibrium, then pass N2, and then filter and wash with deionized water in sequence, and finally place in a drying oven at 70 to 75° C. and dry for 10 to 12 hours to obtain the chlorinated regenerated rubber.
[0020] Preferably, the antioxidant is selected from saturated octadecylamide or 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole; the plasticizer is selected from one or more of diisooctyl phthalate, dimethyl phthalate, diethyl phthalate, diisononyl phthalate and diisodecyl phthalate.
[0021] A method for preparing an aviation cable coating material comprises the following preparation steps:
[0022] Step 1, weigh each raw material according to weight;
[0023] Step 2: Put the polyethylene resin and the chlorinated regenerated rubber into a kneader and knead them at 80-100° C. for 10 minutes;
[0024] Step 3: Add flame retardant, thermal conductive filler, antioxidant and plasticizer, stir evenly, put into a twin-screw extruder for melt extrusion, air-cooling and granulation, and obtain aviation cable covering material. Beneficial Effects
[0025] The present invention provides an aviation cable coating material and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The aviation cable coating material and its preparation method are characterized in that the attapulgite is modified so that it can be better dispersed in the matrix, and a small amount of doping is used to provide more hard units. The specific optical density of the modified attapulgite is improved, so that when the material is burned, it provides a tighter carbon layer, inhibits the release of smoke and blocks the entry of oxygen, inhibits surface combustion, and thus achieves the effect of smoke suppression and flame retardancy. At the same time, the modified attapulgite acts as a nano-reinforcement material and acts as a nano-rebar in the material, which significantly improves the fracture strength of the material.
[0027] (2) The aviation cable coating material and its preparation method are characterized by mixing alkali-treated hexagonal boron nitride with treated spherical alumina, so that the treated spherical alumina can be well coated on the surface of the hexagonal boron nitride, thereby constructing more heat conduction channels in the material, improving the thermal conductivity of the material, and effectively reducing the operating temperature of the cable, thereby improving the service life and safety of the cable; at the same time, since the added thermal conductive filler is a rigid particle, when the material is stretched by an external force, the thermal conductive filler will enhance the material, thereby increasing the tensile strength of the material.
[0028] (3) The aviation cable coating material and its preparation method, by adding chlorinated recycled rubber, forms a firm charred layer on the surface of the material after combustion. The formation of the charred layer can effectively prevent the transfer of heat and flammable volatiles between the flame area and the substrate, thereby preventing continued combustion and producing good flame retardancy. At the same time, it can also effectively improve the aging resistance of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 SEM images of the carbon layer after combustion of the materials of Example 1 and Comparative Example 2 provided for an aviation cable coating material and a preparation method thereof of the present invention;
[0030] Figure 2 The present invention provides an aviation cable coating material and a preparation method thereof, and provides a SEM image of a mixture of hexagonal boron nitride and spherical alumina before and after treatment.
[0031] Figure 2 Middle: a is the SEM image of the mixture of hexagonal boron nitride and spherical alumina before treatment, b is the SEM image of a magnified 20 times; c is the SEM image of the mixture of hexagonal boron nitride and spherical alumina after treatment, d is the SEM image of c magnified 20 times. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] In the technical scheme, the specific alkali treatment method of hexagonal boron nitride is: add 300mL of 5mol / L sodium hydroxide solution to 12g of hexagonal boron nitride, heat to boiling after mixing, reflux and stir, wash with distilled water until neutral, and place in a vacuum drying oven at 90°C for drying.
[0034] The specific method for pretreatment of the surface of spherical alumina is as follows: KH550 and distilled water are mixed in a molar ratio of 1:3 to obtain a mixed solution 1; KH550 and anhydrous ethanol are mixed in a volume ratio of 1:1 to obtain a mixed solution 2; the mixed solution 1 is mixed with the mixed solution 2, and the mixture is heated to 35°C in a water bath, and the reaction is carried out for 40 minutes to obtain a hydrolyzate; the hydrolyzate is divided into three parts, and the parts are poured into a mixer containing spherical alumina in turn, and the mixture is heated to 115°C and stirred. Example 1
[0035] A method for preparing an aviation cable coating material comprises the following preparation steps:
[0036] Step 1, weigh the raw materials according to weight: 100g polyethylene resin, 45g chlorinated recycled rubber, 2g modified attapulgite, 2.5g thermal conductive filler, 4g saturated octadecamide, and 6g diisooctyl phthalate;
[0037] The specific modification method of the modified attapulgite is as follows: 97 g of attapulgite is ground into powder and then placed in a drying oven at 70 ° C for 10 hours; taken out, 1 g of TM931 is added thereto at room temperature, first stirred at a speed of 300 r / min for 5 minutes, and after a mixture of lumpy particles and powder exists, stirred at a high speed of 20000 r / min for 2 minutes, and then allowed to stand for 1 minute, and the operation is repeated 3 times to obtain the modified attapulgite;
[0038] The preparation method of the thermal conductive filler is as follows: placing the hexagonal boron nitride after alkali treatment and the spherical aluminum oxide after surface pretreatment in ethanol at a mass ratio of 1:2.5, and ultrasonically treating for 30 minutes; stirring and mixing the two solutions to obtain the thermal conductive filler;
[0039] The preparation method of chlorinated regenerated rubber is as follows: pour 500 mL of distilled water into 90 g of regenerated rubber particles, heat to 70°C and stir, then add 0.6 g of azobisisobutyronitrile, pass Cl2, pass N2 until the chlorine content reaches equilibrium, then filter and wash with deionized water in sequence, and finally dry in a drying oven at 70°C for 10 hours to obtain chlorinated regenerated rubber;
[0040] Step 2: Put the polyethylene resin and the chlorinated regenerated rubber into a kneader and knead them at 80° C. for 10 minutes;
[0041] Step 3: Add flame retardant, thermal conductive filler, antioxidant and plasticizer, stir evenly, put into a twin-screw extruder for melt extrusion, air-cooling and granulation, and obtain aviation cable covering material. Example 2
[0042] A method for preparing an aviation cable coating material comprises the following preparation steps:
[0043] Step 1, weigh the raw materials according to weight: 110g polyethylene resin, 40g chlorinated recycled rubber, 1.4g modified attapulgite, 2g thermal conductive filler, 2.5g 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 4g dimethyl phthalate;
[0044] The specific modification method of the modified attapulgite is as follows: 98 g of attapulgite is ground into powder and then placed in a drying oven at 75°C for 11 hours; taken out, 1 g of TM931 is added thereto at room temperature, first stirred at a speed of 400 r / min for 6 minutes, and after a mixture of lumpy particles and powder exists, stirred at a high speed of 24000 r / min for 3 minutes, and then allowed to stand for 1 minute, and the operation is repeated 3 times to obtain the modified attapulgite;
[0045] The preparation method of the thermal conductive filler is as follows: placing the hexagonal boron nitride after alkali treatment and the spherical aluminum oxide after surface pretreatment in ethanol at a mass ratio of 1:2.8, and ultrasonically treating for 35 minutes; stirring and mixing the two solutions to obtain the thermal conductive filler;
[0046] The preparation method of chlorinated regenerated rubber is as follows: pour 500 mL of distilled water into 95 g of regenerated rubber particles, heat to 75° C. and stir, then add 0.8 g of azobisisobutyronitrile, pass Cl2, pass N2 until the chlorine content reaches equilibrium, then filter and wash with deionized water in sequence, and finally dry in a drying oven at 75° C. for 10 to 12 hours to obtain chlorinated regenerated rubber;
[0047] Step 2: Put the polyethylene resin and the chlorinated regenerated rubber into a kneader and knead them at 90° C. for 10 minutes;
[0048] Step 3: Add flame retardant, thermal conductive filler, antioxidant and plasticizer, stir evenly, put into a twin-screw extruder for melt extrusion, air-cooling and granulation, and obtain aviation cable covering material. Example 3
[0049] A method for preparing an aviation cable coating material comprises the following preparation steps:
[0050] Step 1, weigh the raw materials according to weight: 120g polyethylene resin, 35g chlorinated regenerated rubber, 0.8g modified attapulgite, 1.5g thermal conductive filler, 1g saturated octadecamide, 2g diisononyl phthalate;
[0051] The specific modification method of the modified attapulgite is as follows: 99 g of attapulgite is ground into powder and then placed in a drying oven at 80 ° C for 12 hours; taken out, 1 g of TM931 is added thereto at room temperature, first stirred at a speed of 500 r / min for 8 minutes, and after a mixture of agglomerated particles and powder exists, stirred at a high speed of 25000 r / min for 3 minutes, and then allowed to stand for 2 minutes, and the operation is repeated 3 times to obtain the modified attapulgite;
[0052] The preparation method of the thermal conductive filler is as follows: the hexagonal boron nitride after alkali treatment and the spherical aluminum oxide after surface pretreatment are placed in ethanol in a mass ratio of 1:3, and ultrasonically treated for 40 minutes; the two solutions are stirred and mixed to obtain the thermal conductive filler;
[0053] The preparation method of chlorinated regenerated rubber is as follows: pour 500 mL of distilled water into 100 g of regenerated rubber particles, heat to 80° C. and stir, then add 0.9 g of azobisisobutyronitrile, pass Cl2, pass N2 until the chlorine content reaches equilibrium, then filter and wash with deionized water in sequence, and finally dry in a drying oven at 75° C. for 12 hours to obtain chlorinated regenerated rubber;
[0054] Step 2: Put the polyethylene resin and the chlorinated regenerated rubber into a kneader and knead them at 100° C. for 10 minutes;
[0055] Step 3: Add flame retardant, thermal conductive filler, antioxidant and plasticizer, stir evenly, put into a twin-screw extruder for melt extrusion, air-cooling and granulation, and obtain aviation cable covering material.
[0056] Comparative Example 1
[0057] Compared with Example 1, the chlorinated regenerated rubber in Example 1 is replaced by regenerated rubber.
[0058] Comparative Example 2
[0059] Compared with Example 1, the modified attapulgite in Example 1 was replaced with attapulgite.
[0060] Comparative Example 3
[0061] Compared with Example 1, the thermal conductive filler in Example 1 is replaced by a mixture of hexagonal boron nitride and spherical aluminum oxide.
[0062] Mechanical properties test: The tensile strength and elongation at break of the material were measured at a rate of 25 mm / min according to GB / T2951.11-2008. The impact strength of the material was measured using an impact testing machine from Shenzhen Xinsansi according to GB / T1843-2008. The results are shown in Table 1.
[0063] LOI determination: According to ISO4589-2:2096 standard, the LOI of the sample was tested using a JF-5 fully automatic oxygen index meter. The sample size was 100 mm × 6.5 mm × 3.0 mm. The results are shown in Table 1.
[0064] Thermal conductivity test: The thermal conductivity of the sample at room temperature was measured by transient hot wire method using a TC3000 thermal conductivity meter from Xi’an Xiaxi Electronic Technology Co., Ltd. In this method, a thin metal wire probe as a linear heat source and temperature sensor was placed between two 2 mm thick flat test specimens; the results are shown in Table 1.
[0065] Table 1
[0066]
[0067] Aging resistance test: The specimens were placed in an aging box for testing. The specimens were dumbbell-shaped. The temperature was set to 150°C for 120 hours. The test was conducted according to the method specified in GB / T2941-2006. The results are shown in Table 2.
[0068] Table 2
[0069]
[0070] like Figure 1 As shown, the carbon layer on the surface of the material of Comparative Example 2 is discontinuous and has gaps, which is one of the spaces for the exchange of oxygen and combustibles; the carbon layer of the material of Example 1 is denser and continuous, and there are no large gaps. The attapulgite has thermal response, and decomposes when heated and is enriched on the surface of the material, blocking the entry of thermal radiation and oxygen. The formation of this barrier layer blocks the exchange of matter and heat between the material itself and the outside world, thereby improving the flame retardant properties of the material.
[0071] like Figure 2 As shown, the treated spherical alumina is well coated on the surface of hexagonal boron nitride to form a spherical alumina-coated hexagonal boron nitride structure, thereby constructing more heat conduction channels in the material, improving the thermal conductivity of the material, and effectively reducing the operating temperature of the cable and improving the service life and safety of the cable.
[0072] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.
[0073] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0074] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An aviation cable coating material, characterized in that: The aviation cable coating material comprises the following components in parts by weight: 100-120 parts of polyethylene resin, 35-45 parts of chlorinated regenerated rubber, 0.8-2 parts of flame retardant, 1.5-2.5 parts of thermal conductive filler, 1-4 parts of anti-aging agent, and 2-6 parts of plasticizer; The flame retardant is modified attapulgite, and the specific modification method is: (1) Grind the attapulgite into powder and dry it in a drying oven at 70 to 80°C for 10 to 12 hours; (2) taking out, adding a titanate coupling agent thereto at room temperature, stirring and mixing, and obtaining a modified attapulgite; The preparation method of the thermal conductive filler is: Ⅰ. Alkali treatment of hexagonal boron nitride; Ⅱ. Pre-treating the surface of spherical alumina; III. Place the treated hexagonal boron nitride and spherical alumina in ethanol at a mass ratio of 1:(2.5-3) and perform ultrasonic treatment for 30-40 minutes; IV. Stir and mix the two solutions to obtain a thermally conductive filler; In the above II, the specific method for pretreating the surface of spherical alumina is as follows: KH550 is mixed with distilled water to obtain a mixed solution 1; KH550 is mixed with anhydrous ethanol to obtain a mixed solution 2; the mixed solution 1 is mixed with the mixed solution 2, and the mixture is heated to 30-35°C in a water bath, and the mixture is reacted for 30-40 minutes to obtain a hydrolyzate; the hydrolyzate is divided into three parts, and the parts are poured into a mixer containing spherical alumina in sequence, and the mixture is heated to 105-115°C and stirred; The preparation method of the chlorinated regenerated rubber is as follows: pour 500 mL of distilled water into 90-100 g of regenerated rubber particles, heat to 70-80° C. and stir, then add 0.6-0.9 g of azobisisobutyronitrile, pass Cl2, pass N2 until the chlorine content reaches equilibrium, filter and wash with deionized water in sequence, and finally place in a drying oven at 70-75° C. and dry for 10-12 hours to obtain the chlorinated regenerated rubber.
2. The aviation cable coating material according to claim 1, characterized in that: The mass ratio of the attapulgite to the titanate coupling agent is (97-99):1, and the titanate coupling agent is TM931.
3. The aviation cable coating material according to claim 1, characterized in that: In the above (2), the specific stirring method is: first stirring at a speed of 300-500 r / min for 5-8 min, and after a mixture of agglomerated particles and powder exists, stirring at a high speed of 20000-25000 r / min for 2-3 min, and then standing for 1-2 min, and repeating the operation 3 times.
4. The aviation cable coating material according to claim 1, characterized in that: In said Ⅰ, the specific alkali treatment method of hexagonal boron nitride is: add 280-300mL of 5mol / L sodium hydroxide solution to 10-12g of hexagonal boron nitride, heat to boiling after mixing, reflux and stir, wash with distilled water until neutral, and dry in a vacuum drying oven at 85-90°C.
5. The aviation cable coating material according to claim 1, characterized in that: The molar ratio of KH550 to distilled water is 1:(2.6-3), and the volume ratio of KH550 to anhydrous ethanol is 1:(0.9-1).
6. The aviation cable coating material according to claim 1, characterized in that: The antioxidant is selected from saturated octadecylamide or 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole; the plasticizer is selected from one or more of diisooctyl phthalate, dimethyl phthalate, diethyl phthalate, diisononyl phthalate and diisodecyl phthalate.
7. A method for preparing an aviation cable coating material according to claim 1, characterized in that: The method comprises the following preparation steps: Step 1, weigh each raw material according to weight; Step 2: Put the polyethylene resin and the chlorinated regenerated rubber into a kneader and knead them at 80-100° C. for 10 minutes; Step 3: Add flame retardant, thermal conductive filler, antioxidant and plasticizer, stir evenly, put into a twin-screw extruder for melt extrusion, air-cooling and granulation, and obtain aviation cable covering material.