Preparation method of nano silicon dioxide composite material
By using naphthyl hyperbranched polyamide ester and TDI modified nano-silica in PET/PA6 alloy materials, the problem of poor compatibility between nano-silica and PET and PA6 is solved, and the mechanical properties of the alloy materials are improved. and heat resistance, achieving better dispersion and thermal stability.
Patent Information
- Application Number
- CN202411049080.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-15
AI Technical Summary
Nano-silica has poor compatibility with polyethylene terephthalate (PET) and polyamide 6 (PA6), resulting in poor mechanical properties and heat resistance of PET/PA6 alloy materials.
Naphthyl hyperbranched polyamide ester and modified nanosilica are used to prepare naphthyl AB2 monomer through acid chloride esterification reaction and nitro reduction reaction. The hyperbranched polyamide ester is obtained by self-polymerization and is extruded in a twin-screw extruder. It is blended with PET and PA6, and TDI modified nano-silica is added to improve compatibility and dispersion.
It significantly improves the tensile properties, impact strength and heat resistance of PET/PA6 alloy materials, improves the compatibility between nano-silica and PET and PA6, and delays the thermal decomposition temperature of the material.
Smart Images

Figure BDA0004974364570000021 
Figure BDA0004974364570000031 
Figure BDA0004974364570000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano silicon dioxide, and specifically relates to a method for preparing a nano silicon dioxide composite material. Background Art
[0002] Nano-silicon dioxide is a common inorganic nano-material with large specific surface area, high mechanical strength and strong high temperature resistance. It can improve the mechanical strength and heat resistance of materials and is widely used in polymer materials such as plastics and rubber. The key is to modify the surface of nano-silicon dioxide, overcome its agglomeration and improve its compatibility with polymer materials.
[0003] Hyperbranched polymers are functional materials with dendritic three-dimensional molecular chains and contain a large number of active functional groups at the ends. They can be used as processing aids and toughening agents to improve the processing properties, mechanical properties and other properties of materials. They have a wide range of practical applications in materials such as PET and nylon 6.
[0004] Polyethylene terephthalate (PET) is non-toxic and tasteless, has good sanitation and safety, good chemical resistance, high transparency, and good gloss. It is widely used in the electronics, packaging, and automotive industries. In order to improve the mechanical strength and heat resistance of PET, it is usually necessary to add modifiers such as nano-silica and glass fiber.
[0005] By blending polyethylene terephthalate with materials such as nylon 6, polyethylene, and polypropylene, an alloy material with better performance can be obtained. It is usually necessary to add a compatibilizer to improve the compatibility between PET and nylon 6, polyethylene, etc. The patent with announcement number CN103073853B discloses a low-cost, low-water-absorption, easy-to-form PA / PET alloy material and preparation method, using PA6 film recycled material, PET recycled material, high-temperature resistant polyamide recycled material, etc. as raw materials, Exxelor TMVA1840, etc. as a compatibilizer, improving the high water absorption rate of PA materials and the shortcomings of slow cooling of PET, while solving the problem of poor compatibility between the two. However, the patent improves the problem of poor compatibility between nano-silica and PET and PA6, and does not significantly improve the mechanical properties such as tensile strength of PA / PET alloy materials. Summary of the invention
[0006] The invention provides a method for preparing a nano silicon dioxide composite material, which solves the problem of poor compatibility among nano silicon dioxide, PET and PA6, and improves the mechanical properties and heat resistance of the PET / PA6 alloy material.
[0007] Technical solution: A method for preparing a nano-silicon dioxide composite material:
[0008] Step A: nitrogen is introduced into a reaction vessel, N-methylpyrrolidone, naphthyl AB2 monomer, triphenyl phosphite, and pyridine are added, and the polymerization reaction is carried out by stirring, and the reaction is cooled, and methanol is added to precipitate the precipitate, and the precipitate is washed with ethanol after filtering and drying to obtain naphthyl hyperbranched polyamide ester. The reaction formula is as follows:
[0009]
[0010] Step B: adding 60-80 parts by weight of polyethylene terephthalate, 20-40 parts by weight of nylon 6, 3-15 parts by weight of naphthyl hyperbranched polyamide ester, and 0.5-5 parts by weight of TDI-modified nano-silicon dioxide into a twin-screw extruder for extrusion granulation to obtain a nano-silicon dioxide composite material.
[0011] Preferably, the amount of naphthyl AB2 monomer used is 100 parts by weight, the amount of triphenyl phosphite is 115-122 parts by weight, and the amount of pyridine is 90-110 parts by weight.
[0012] Preferably, the polymerization reaction is carried out at 90-110° C. for 3-5 h.
[0013] Preferably, the temperature of sections 1-6 of the twin-screw extruder is 225-260°C.
[0014] Preferably, the preparation method of naphthyl AB2 monomer is:
[0015] Step (1), adding toluene or tetrahydrofuran solvent, 150-165 parts by weight of 2-hydroxy-6-naphthoic acid, 65-78 parts by weight of pyridine into a reaction container, adding 100 parts by weight of 5-nitroisophthaloyl chloride under ice bath, and then stirring and reacting at 15-35° C. for 12-18 hours, distilling off the solvent under reduced pressure, separating by silica gel column chromatography, and using a mixed solution of ethyl acetate and petroleum ether as the eluent to obtain 5-nitroisophthalic acid naphthoate.
[0016] Step (2), add concentrated hydrochloric acid, 100 parts by weight of 5-nitroisophthalate naphthoic acid, and 80-92 parts by weight of tin powder to a reaction vessel equipped with a condenser reflux tube, carry out reduction reaction at 70-85°C for 2-4h, add water to dilute, add ammonia water to neutralize, filter and extract the filtrate with ethyl acetate, dry the organic phase to remove water, distill under reduced pressure, separate the crude product by silica gel column chromatography, and the eluent is a mixed solution of ethyl acetate and petroleum ether to obtain a naphthyl AB2 monomer. The preparation reaction formula is as follows:
[0017]
[0018] Preferably, the preparation method of TDI modified nano-silica is: adding toluene and nano-silica into a reaction container, ultrasonically dispersing, adding toluene-2,4-diisocyanate, stirring for reaction, centrifugal separation, washing with acetone, and drying to obtain TDI modified nano-silica.
[0019] Technical effect: The present invention uses 2-hydroxy-6-naphthoic acid and 5-nitroisophthaloyl chloride as raw materials, and obtains a novel naphthyl AB2 monomer containing one amino group and two carboxyl groups through an acyl chloride esterification reaction and a nitro reduction reaction. The naphthyl hyperbranched polyamide ester is obtained through a self-polymerization reaction.
[0020] The invention adds naphthyl hyperbranched polyamide ester and TDI modified nano silicon dioxide into the PET and nylon 6 alloy composite material. The hyperbranched polyamide ester contains an ester structural unit and an amide bond structural unit, while PET also contains an ester structural unit and nylon 6 contains an amide bond structural unit, so that the naphthyl hyperbranched polyamide ester has good compatibility with both PET and nylon 6, and the naphthyl hyperbranched polyamide ester can be used as a compatibilizer to improve the interface compatibility between PET and nylon 6.
[0021] After the nano silicon dioxide of the present invention is modified by TDI, the dispersibility is very good and it is not easy to agglomerate in the alloy composite material matrix; and the terminal amino group contained in the naphthyl hyperbranched polyamide ester can react with the isocyanate group on the surface of the modified nano silicon dioxide, so that the hyperbranched polyamide ester is grafted to the surface of the modified nano silicon dioxide, and the compatibility between the nano silicon dioxide and PET and nylon 6 is further improved. Under the synergistic effect, the tensile property and impact strength of the alloy composite material are improved, and the composite material has better mechanical properties. In addition, the hyperbranched polyamide ester contains a naphthalene ring structure with high temperature resistance, is not easy to be thermally decomposed, and is added to the alloy composite material to increase the material quality loss temperature, so that the composite material has better heat resistance. DETAILED DESCRIPTION
[0022] The following will clearly and completely describe the concept of the present application and the technical effects produced in combination with the embodiments, so as to fully understand the purpose, features and effects of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of them. Based on the embodiments of the present application, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present application.
[0023] The polyethylene terephthalate of the present invention has a model of CB-602, a brand of nylon 6 of 1013B, an average particle size of nano silicon dioxide of 30 nm, a CAS registration number of 2-hydroxy-6-naphthoic acid of 16712-64-4, and a CAS registration number of 5-nitroisophthaloyl chloride of 13438-30-7.
[0024] Example 1
[0025] (1) Add 80 mL of toluene and 5 g of nano-silica into a reaction container, disperse by ultrasonication, add 4 g of toluene-2,4-diisocyanate, stir and react at 90° C. for 2 h, centrifuge, wash with acetone, and dry to obtain TDI-modified nano-silica.
[0026] (2) Add 150 mL of toluene solvent, 15 g of 2-hydroxy-6-naphthoic acid, and 7.2 g of pyridine to a reaction vessel, add 10 g of 5-nitroisophthaloyl chloride under ice bath, and then stir and react at 35° C. for 12 h. Distill under reduced pressure to remove the solvent, separate by silica gel column chromatography, and use a mixed solution of ethyl acetate and petroleum ether as the eluent to obtain 5-nitroisophthalic acid naphthoate.
[0027] (3) Add 60 mL of 36% concentrated hydrochloric acid, 20 g of 5-nitroisophthalic acid naphthoic acid, and 16 g of tin powder to a reaction vessel equipped with a condenser reflux tube, and carry out a reduction reaction at 70° C. for 4 h. Add water to dilute, add ammonia water to neutralize, filter, extract the filtrate with ethyl acetate, dry the organic phase to remove water, and distill under reduced pressure. The crude product is separated by silica gel column chromatography, and the eluent is a mixed solution of ethyl acetate and petroleum ether to obtain a naphthyl AB2 monomer.
[0028] (4) nitrogen was introduced into the reaction vessel, 100 mL of N-methylpyrrolidone, 20 g of naphthyl AB2 monomer, 24.4 g of triphenyl phosphite, and 21 g of pyridine were added, and the polymerization reaction was carried out at 90° C. with stirring for 5 h. The mixture was cooled, and methanol was added to precipitate the precipitate. The precipitate was filtered and washed with ethanol, and then dried to obtain naphthyl hyperbranched polyamide ester.
[0029] (5) Add 800 g of polyethylene terephthalate, 200 g of nylon 6, 30 g of naphthyl hyperbranched polyamide ester, and 5 g of TDI-modified nano-silica into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0030] Example 2
[0031] (1) Add 200 mL of tetrahydrofuran solvent, 16.5 g of 2-hydroxy-6-naphthoic acid, and 6.5 g of pyridine to a reaction container, add 10 g of 5-nitroisophthaloyl chloride under ice bath, and then stir and react at 35° C. for 12 h. Distill under reduced pressure to remove the solvent, separate by silica gel column chromatography, and use a mixed solution of ethyl acetate and petroleum ether as the eluent to obtain 5-nitroisophthalic acid naphthoate.
[0032] (2) Add 80 mL of 36% concentrated hydrochloric acid, 20 g of 5-nitroisophthalic acid naphthoic acid, and 18.4 g of tin powder to a reaction vessel equipped with a condenser reflux tube, and carry out a reduction reaction at 85° C. for 2 h. Add water to dilute, add ammonia water to neutralize, filter, extract the filtrate with ethyl acetate, dry the organic phase to remove water, and distill under reduced pressure. The crude product is separated by silica gel column chromatography, and the eluent is a mixed solution of ethyl acetate and petroleum ether to obtain a naphthyl AB2 monomer.
[0033] (3) nitrogen was introduced into the reaction vessel, 100 mL of N-methylpyrrolidone, 20 g of naphthyl AB2 monomer, 23 g of triphenyl phosphite, and 22 g of pyridine were added, and the polymerization reaction was carried out at 90° C. with stirring for 5 h. The mixture was cooled, and methanol was added to precipitate the precipitate. The precipitate was filtered and washed with ethanol, and then dried to obtain naphthyl hyperbranched polyamide ester.
[0034] (4) Add 700 g of polyethylene terephthalate, 300 g of nylon 6, 30 g of naphthyl hyperbranched polyamide ester, and 25 g of TDI-modified nano-silica (prepared in Example 1) into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0035] Example 3
[0036] (1) Add 150 mL of toluene solvent, 15 g of 2-hydroxy-6-naphthoic acid, and 7.8 g of pyridine to a reaction vessel, add 10 g of 5-nitroisophthaloyl chloride under ice bath, and then stir and react at 15° C. for 18 h. Distill under reduced pressure to remove the solvent, separate by silica gel column chromatography, and use a mixed solution of ethyl acetate and petroleum ether as the eluent to obtain 5-nitroisophthalic acid naphthoate.
[0037] (2) Add 80 mL of 36% concentrated hydrochloric acid, 20 g of 5-nitroisophthalic acid naphthoic acid, and 17.6 g of tin powder to a reaction vessel equipped with a condenser reflux tube, and carry out a reduction reaction at 80° C. for 2 h. Add water to dilute, add ammonia water to neutralize, filter, extract the filtrate with ethyl acetate, dry the organic phase to remove water, and distill under reduced pressure. The crude product is separated by silica gel column chromatography, and the eluent is a mixed solution of ethyl acetate and petroleum ether to obtain a naphthyl AB2 monomer.
[0038] (3) nitrogen was introduced into the reaction vessel, 100 mL of N-methylpyrrolidone, 20 g of naphthyl AB2 monomer, 24.4 g of triphenyl phosphite, and 18 g of pyridine were added, and the polymerization reaction was carried out at 110° C. with stirring for 5 h. The reaction was cooled, methanol was added to precipitate, the precipitate was filtered and washed with ethanol, and dried to obtain naphthyl hyperbranched polyamide ester.
[0039] (4) Add 800 g of polyethylene terephthalate, 200 g of nylon 6, 30 g of naphthyl hyperbranched polyamide ester, and 50 g of TDI-modified nano-silica (prepared in Example 1) into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0040] Comparative Example 1
[0041] The difference between this comparative example and Example 1 is that the naphthyl hyperbranched polyamide ester and TDI-modified nano-silica are not added.
[0042] 800 g of polyethylene terephthalate and 200 g of nylon 6 were extruded into granules in a twin-screw extruder. The temperatures of sections 1-6 were 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a PET / PA6 alloy composite material.
[0043] Comparative Example 2
[0044] The difference between this comparative example and Example 1 is that no naphthyl hyperbranched polyamide ester is added, and unmodified nano-silica is added.
[0045] 800 g of polyethylene terephthalate, 200 g of nylon 6 and 5 g of nano-silicon dioxide were added into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 were 225° C., 240° C., 260° C., 260° C., 255° C. and 250° C. to obtain a PET / PA6 alloy composite material.
[0046] Comparative Example 3
[0047] The difference between this comparative example and Example 1 is that no naphthyl hyperbranched polyamide ester is added.
[0048] 800 g of polyethylene terephthalate, 200 g of nylon 6, and 5 g of TDI-modified nano-silica were added into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 were 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a PET / PA6 alloy composite material.
[0049] Comparative Example 4
[0050] The difference between this comparative example and Example 1 is that no TDI-modified nano-silica is added.
[0051] 800 g of polyethylene terephthalate, 200 g of nylon 6, and 30 g of naphthyl hyperbranched polyamide ester were added to a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 were 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a PET / PA6 alloy composite material.
[0052] Comparative Example 5
[0053] The difference between this comparative example and Example 1 is that unmodified nano-silicon dioxide is added.
[0054] 800 g of polyethylene terephthalate, 200 g of nylon 6, 30 g of naphthyl hyperbranched polyamide ester and 5 g of nano-silicon dioxide were added into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 were 225° C., 240° C., 260° C., 260° C., 255° C. and 250° C. to obtain a PET / PA6 alloy composite material.
[0055] The composite material was injection molded in an injection molding machine, and the temperatures of the barrel of the injection molding machine were 235°C, 245°C, 245°C, and 240°C; samples were injection molded and performance tested.
[0056] The tensile properties of the composite materials were tested according to GB / T 1040.1-2018 method, with a sample size of 100 mm × 10 mm × 5 mm. The tensile rate was 5 mm / min; 5 samples were tested in each group and the average value was taken.
[0057] The notched impact strength was tested according to GB / T 1043.1-2008 method. The sample size was 100mm×10mm×4mm. Five samples were tested in each group and the average value was taken.
[0058] The thermal properties of the samples were tested using a thermogravimetric analyzer, with a sample size of 5 mg, a test temperature range of 30-700°C, a heating rate of 10°C / min, and a nitrogen atmosphere. The test results are shown in the table below.
[0059]
[0060]
[0061] As can be seen from the table above, Comparative Example 1 is an alloy composite material of polyethylene terephthalate and nylon 6. Since no compatibilizer is added, the compatibility between the two is poor, resulting in low tensile strength, elongation at break and impact strength of the composite material, and poor mechanical properties. In addition, the temperature at which the mass loss is 5% and the temperature at which the decomposition rate is the maximum are low, and the heat resistance is poor.
[0062] The PET and nylon 6 alloy composite materials of embodiments 1-3 are added with naphthyl hyperbranched polyamide ester and TDI modified nano-silicon dioxide. Hyperbranched polyamide ester contains ester structural units and amide bond structural units, while PET also contains ester structural units, and nylon 6 contains amide bond structural units, so that the naphthyl hyperbranched polyamide ester has good compatibility with both PET and nylon 6, and the naphthyl hyperbranched polyamide ester can be used as a compatibilizer to improve the interface compatibility between PET and nylon 6. At the same time, after the nano-silicon dioxide is modified by TDI, the dispersibility is very good, and it is not easy to agglomerate in the material matrix; and the terminal amino group contained in the naphthyl hyperbranched polyamide ester can react with the isocyanate group on the surface of the modified nano-silicon dioxide, so that the hyperbranched polyamide ester is grafted to the surface of the modified nano-silicon dioxide, further improving the compatibility between the nano-silicon dioxide and PET and nylon 6. Under the synergistic effect, the tensile properties and impact strength of the alloy composite material are improved, and it has better mechanical properties. In addition, the hyperbranched polyamide ester contains a high-temperature-resistant naphthalene ring structure, which can be added to the alloy composite material to improve its heat resistance, and the temperature at which the mass loss is 5% and the temperature at which the decomposition rate is maximum are significantly increased.
[0063] Comparative Example 2 added unmodified nano-silica. The compatibility between nano-silica and polyethylene terephthalate and nylon 6 is poor, the dispersibility in the PET / PA6 alloy composite is poor, and it is easy to agglomerate. The mechanical properties and heat resistance of the alloy composite are not significantly improved. Compared with Comparative Example 1, the increase in its tensile properties, impact strength and thermal decomposition temperature is lower.
[0064] After the nano-silica in Comparative Example 3 is surface-modified with TDI toluene-2,4-diisocyanate, the dispersibility of the nano-silica can be improved, the agglomeration in the alloy composite material can be reduced, the tensile properties and impact strength are significantly improved, and the mechanical properties of the composite material are better, which are significantly higher than those of Comparative Example 1. However, without the addition of naphthyl hyperbranched polyamide ester, the mechanical properties and heat resistance performance are lower than those of Example 1.
[0065] Comparative Example 4 adds naphthyl hyperbranched polyamide ester, which can be used as a compatibilizer to improve the interface compatibility between PET and nylon 6, so that the alloy composite material has better mechanical properties and heat resistance, and the tensile properties, impact strength, temperature at 5% mass loss and temperature at maximum decomposition rate are higher than those in Comparative Example 1. However, no TDI-modified nano-silica is added, and the mechanical properties and heat resistance are lower than those in Example 1.
[0066] In Comparative Example 5, unmodified nano-silica and naphthyl hyperbranched polyamide ester were added. The nano-silica had poor dispersibility and was prone to agglomeration. It did not contain isocyanate groups and could not react with the terminal amino groups of the naphthyl hyperbranched polyamide ester. It had poor compatibility with PET and PA6 and could not effectively improve the mechanical properties of the material. The tensile properties and impact strength were lower than those in Example 1.
[0067] Example 1 and Comparative Example 5 both added naphthyl hyperbranched polyamide ester, the difference between the two is whether the surface of nano silicon dioxide is modified by TDI. Compared with Comparative Example 5, the increase in tensile strength of Example 1 is (69.1-58.7) / 58.7=17.72%, and the increase in elongation at break is (482.2-430.4) / 430.4=12.04%. The increase in impact strength is (4.92-4.24) / 4.24=16.04%.
[0068] The difference between Comparative Example 2 and Comparative Example 3 is whether the surface of nano-silicon dioxide is modified by TDI. Compared with Comparative Example 2, the increase in tensile strength of Comparative Example 3 is (56.9-52.8) / 52.8=7.77%, and the increase in elongation at break is (402.6-385.0) / 385.0=4.57%. The increase in impact strength is (4.05-3.79) / 3.79=6.86%. The increase in Comparative Example 3 is significantly lower than that in Example 1. This is mainly because Example 1 adds naphthyl hyperbranched polyamide ester, whose terminal amino group can react with the isocyanate group on the surface of modified nano-silicon dioxide, thereby grafting hyperbranched polyamide ester to the surface of modified nano-silicon dioxide, further improving the compatibility between nano-silicon dioxide and PET and nylon 6. TDI modified nano-silicon dioxide plays a better reinforcing role, thereby improving the increase in mechanical properties.
[0069] Example 4
[0070] (1) Add 700 g of polyethylene terephthalate, 300 g of nylon 6, 70 g of naphthyl hyperbranched polyamide ester (prepared in Example 2), and 25 g of TDI-modified nano-silica (prepared in Example 1) into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0071] Example 5
[0072] (1) Add 700 g of polyethylene terephthalate, 300 g of nylon 6, 110 g of naphthyl hyperbranched polyamide ester (prepared in Example 2), and 25 g of TDI-modified nano-silica (prepared in Example 1) into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0073] Example 6
[0074] (1) Add 700 g of polyethylene terephthalate, 300 g of nylon 6, 150 g of naphthyl hyperbranched polyamide ester (prepared in Example 2), and 25 g of TDI-modified nano-silica (prepared in Example 1) into a twin-screw extruder for extrusion granulation. The temperatures of sections 1-6 are 225° C., 240° C., 260° C., 260° C., 255° C., and 250° C. to obtain a nano-silica composite material.
[0075] The composite material was injection molded into a specimen according to the above method and the performance test was carried out. The test results are shown in the table below.
[0076]
[0077] It can be seen from the above table that as the amount of naphthyl hyperbranched polyamide ester gradually increases, the composite materials show good tensile properties and impact strength, and have a high thermal decomposition temperature and excellent heat resistance.
[0078] The present application is described in detail above in conjunction with the embodiments, but the present application is not limited to the above embodiments, and various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present application. In addition, the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing a nano-silicon dioxide composite material, characterized in that: The preparation method is as follows: Step A: introducing nitrogen into a reaction container, adding N-methylpyrrolidone, naphthyl AB2 monomer, triphenyl phosphite and pyridine, stirring to carry out polymerization reaction, cooling, adding methanol to precipitate the precipitate, filtering, washing and drying to obtain naphthyl hyperbranched polyamide ester; The naphthyl AB2 monomer has the structural formula (I) as follows: Step B: adding 60-80 parts by weight of polyethylene terephthalate, 20-40 parts by weight of nylon 6, 3-15 parts by weight of naphthyl hyperbranched polyamide ester, and 0.5-5 parts by weight of TDI-modified nano-silicon dioxide into a twin-screw extruder for extrusion granulation to obtain a nano-silicon dioxide composite material.
2. The method for preparing the nano-silicon dioxide composite material according to claim 1, characterized in that: The amount of the naphthyl AB2 monomer used is 100 parts by weight, the amount of triphenyl phosphite is 115-122 parts by weight, and the amount of pyridine is 90-110 parts by weight.
3. The method for preparing the nano-silicon dioxide composite material according to claim 1, characterized in that: The polymerization reaction is carried out at 90-110° C. for 3-5 hours.
4. The method for preparing the nano-silicon dioxide composite material according to claim 1, characterized in that: The temperature of sections 1-6 of the twin-screw extruder is 225-260°C.
5. The method for preparing the nano-silicon dioxide composite material according to claim 1, characterized in that: The preparation method of the naphthyl AB2 monomer is: Step (1), adding a reaction solvent, 2-hydroxy-6-naphthoic acid, and pyridine to a reaction vessel, adding 5-nitroisophthaloyl chloride under an ice bath, and then stirring the reaction at 15-35° C. for 12-18 hours, distilling under reduced pressure, and separating by silica gel column chromatography to obtain 5-nitroisophthalic acid naphthoate; Step (2), adding concentrated hydrochloric acid, 5-nitroisophthalic acid naphthoic acid, and tin powder to a reaction vessel equipped with a condenser reflux tube to carry out a reduction reaction, adding water to dilute, adding ammonia water to neutralize, filtering, extracting the filtrate, distilling under reduced pressure, and separating the crude product by silica gel column chromatography to obtain a naphthyl AB2 monomer.
6. The method for preparing the nano-silicon dioxide composite material according to claim 5, characterized in that: In the step (1), the amount of 5-nitroisophthaloyl chloride used is 100 parts by weight, the amount of 2-hydroxy-6-naphthoic acid used is 150-165 parts by weight, and the amount of pyridine used is 65-78 parts by weight.
7. The method for preparing the nano-silicon dioxide composite material according to claim 5, characterized in that: In the step (1), the reaction solvent is toluene or tetrahydrofuran.
8. The method for preparing the nano-silicon dioxide composite material according to claim 5, characterized in that: In the step (2), the amount of 5-nitroisophthalate naphthoic acid is 100 parts by weight, and the amount of tin powder is 80-92 parts by weight.
9. The method for preparing the nano-silicon dioxide composite material according to claim 5, characterized in that: In the step (2), the reduction reaction is carried out at 70-85° C. for 2-4 hours.
10. The method for preparing the nano-silicon dioxide composite material according to claim 1, characterized in that: The preparation method of the TDI modified nano silicon dioxide comprises the following steps: adding toluene and nano silicon dioxide into a reaction container, performing ultrasonic dispersion, adding toluene-2,4-diisocyanate, stirring for reaction, centrifugal separation, washing with acetone, and drying to obtain the TDI modified nano silicon dioxide.
Citation Information
Cited By
High-temperature-resistant hydrophobic nano coating protective material and preparation method thereof
CN120005514A